A block polymer based on a brush-like cellulose skeleton, a preparation method thereof, and application as a solid electrolyte
Through the design of brush-shaped cellulose skeleton block polymer, the problem of poor electrochemical performance of solid-state lithium batteries is solved, high thermal stability and low glass transition temperature are achieved, lithium ion migration and battery cycle stability are improved, and high support for high thermal stability is supported. Magnification and efficient charging and discharging.
Patent Information
- Application Number
- CN202211033311.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-08-26
AI Technical Summary
The electrochemical performance of solid-state lithium batteries is poor, the lithium ion transmission energy barrier is high, the chemical stability is insufficient, the battery has poor long-term charging and discharge cycle performance, poor interface performance, and cannot support high-energy-consuming facilities.
Brush-shaped cellulose skeleton block polymer is used as solid electrolyte, and its main chain is cellulose, and the side chain is composed of polyethylene oxide and polyvinyl imidazole block copolymerization. It is synthesized by atom transfer radical polymerization technology to combine polymerization ions. The dual advantages of liquid and ether bonds are adjusted to improve performance.
It achieves high thermal stability, low glass transition temperature, excellent mechanical processing performance and good lithium ion migration, improves the electrochemical window and cycle stability of the battery, and supports high magnification and efficient charging and discharge.
Smart Images

Figure CN115286751B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid electrolytes, and in particular relates to a solid electrolyte based on a brush-like cellulose skeleton block polymer and a preparation method thereof. Background Art
[0002] Solid electrolytes replace electrolytes and separators, which reduces costs to a certain extent, reduces the paths of lithium ion migration, and improves capacity levels. Solid-state lithium batteries have the following important advantages: (1) They have high mechanical properties and good flexibility (Flexible) and can be used in various household appliances and wearable devices such as bracelets, curved screens and other electronic products; (2) Replacing separators reduces production costs and reduces plastic pollution; (3) Some solid-state lithium batteries can be used in special environments; (4) They can be well coordinated and compatible with high specific capacity electrode materials (NCM series positive electrode materials, Mg\Na metal negative electrodes); (5) Wide electrochemical window and low area resistance (ASR).
[0003] Solid electrolytes have the advantages of strong mechanical properties, stable chemical properties, and a wide range of temperature conditions (-60 to 500°C (the electrolyte will freeze, boil or decompose in this range). However, the electrochemical properties of solid materials are poor. First, the energy barrier for lithium ion transmission in solid electrolytes is high, and they can only be used normally in an environment above 60°C; second, the chemical stability is insufficient, the electrochemical window is narrow, and the long-term charge and discharge cycle performance of the battery is poor; third, the interface performance of solid-state lithium batteries is poor, which is manifested in slow charge and discharge efficiency and inability to support high-energy consumption facilities. Therefore, it is necessary to develop solid polymer electrolytes with excellent comprehensive performance to solve these problems. Summary of the invention
[0004] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0005] As one aspect of the present invention, the present invention provides a block polymer based on a brush-like cellulose skeleton, wherein the main chain skeleton is cellulose, and the side chain is composed of polyethylene oxide and polyvinyl imidazole block copolymers, and the general structural formula is:
[0006]
[0007] Among them, x is 40-280, y is 40-280, m is 40-280, and n is 220;
[0008] The preparation method of the brush-like cellulose-based block polymer is characterized by the following steps:
[0009] Step 1, microcrystalline cellulose I a Preparation of cellulose skeleton bromine initiator I by reaction with 2-bromoisobutyryl bromide b ;
[0010]
[0011] Step 2: Under nitrogen atmosphere, the initiator I obtained in step 1 b , copper-based catalyst, ligand and polyethylene glycol methacrylate-CH3 monomer undergo atom transfer radical polymerization to obtain cellulose-based polyethylene oxide polymer I c ;
[0012]
[0013] Step 3: Under a nitrogen atmosphere, the cellulose-based polyethylene oxide polymer I obtained in step 2 is c , a copper-based catalyst, a ligand and 1-vinylimidazole undergo an atom transfer radical polymerization reaction to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer I.
[0014]
[0015] Wherein, in step 1, the mass ratio of microcrystalline cellulose to 2-bromoisobutyryl bromide is 1:10-1:15; in step 2, the catalyst used in the atom transfer radical polymerization reaction is one of cuprous chloride or cuprous bromide; the ligand is selected from one of N,N,N',N",N"-pentamethyldiethylenetriamine, tris(2-dimethylaminoethyl)amine, 1,1,4,7,10,10-hexamethyltriethylenetetramine, and 2,2-bipyridine; the initiator I b , the mass ratio of the copper-based catalyst, the ligand and polyethylene glycol methacrylate-CH3 is 1:0.35:0.7:1; in step 3, the mass ratio of Ic to 1-vinylimidazole is 2:1.
[0016] The brush-like cellulose skeleton block polymer solid electrolyte is prepared by blending the brush-like cellulose-based block polymer I, lithium salt and solvent through a solution casting method.
[0017] The lithium salt is one of lithium bis(trifluoromethanesulfonyl)immonium, lithium trifluoromethanesulfonate, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluorophosphate, and lithium perfluoro-1-butanesulfonate; the solvent is one of acetonitrile and dioxane; and the lithium salt accounts for 5% to 25% of the total mass of the all-solid electrolyte.
[0018] Beneficial effects of the present invention:
[0019] (1) Atom transfer radical polymerization technology can be used to synthesize polymers with specific molecular structures, predetermined molecular weights, and narrow molecular weight distribution indexes. The reaction conditions are mild, the reaction speed is fast, and the efficiency is high.
[0020] (2) Polymeric ionic liquids are used as the main body of the polymer, combining the dual advantages of polymeric ionic liquids and ether bonds. They have the characteristics of high thermal stability and high ionic conductivity. They can also "graft" certain specific functional groups through substitution, addition, etc., or adjust the combination of anions and cations, thereby adjusting their physical and chemical properties to meet different reaction requirements. At the same time, due to the presence of ether bonds, they are usually flexible and can form complexes with electron acceptors or certain inorganic electrolytes.
[0021] (3) The brush-like branched structure makes the polymer less crystalline and has a lower glass transition temperature, which has excellent mechanical processing properties, is conducive to achieving good contact between the electrode and the electrolyte interface, and can promote the migration and transportation of lithium ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0023] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer prepared in Example 1.
[0024] Figure 2 This is a physical picture of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte prepared in Example 1.
[0025] Figure 3 This is the differential scanning calorimetry curve of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte prepared in Example 1.
[0026] Figure 4 This is the Arrhenius curve of the ionic conductivity of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte prepared in Example 1.
[0027] Figure 5 The chronoamperometric curve and AC impedance spectrum of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte prepared in Example 1.
[0028] Figure 6This is the linear sweep voltammetry curve of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte prepared in Example 1.
[0029] Figure 7 This is the charge and discharge curve of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte prepared in Example 1.
[0030] Figure 8 This is a graph of the cycling stability of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte prepared in Example 1.
[0031] Fig. 9 This is a rate performance diagram of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte prepared in Example 1. DETAILED DESCRIPTION
[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.
[0033] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0034] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0035] Embodiment 1: (x is 60-280, y is 80, m is 100)
[0036] In a glove box filled with argon, weigh 2g of microcrystalline cellulose into a round-bottom flask, add 10g of 1-allyl-3-methylimidazole chloride and stir thoroughly, then add 20mL of DMF, the process needs to be added dropwise gradually, the temperature is lowered in a stepwise manner, and finally placed in an ice-water bath for 1h, then 20g of 2-bromoisobutyryl bromide is added dropwise, then the temperature is lowered, placed in an ice-water bath for 15min, and finally stirred at room temperature for 48h. After the stirring is completed, a large amount of deionized water is added to the flask to obtain a white precipitate, and then the white precipitate is dissolved with acetone, and then recrystallized with ethanol. The washing operation is repeated 5 times, and finally vacuum dried in an oven at 70-80°C to obtain a cellulose skeleton bromine initiator.
[0037] Take 0.2g of cellulose skeleton bromine initiator and add 10mL DMF, stir thoroughly for 1.5h, after the white solid is completely dissolved, add 0.2g of polyethylene glycol methacrylate -CH3, 0.14g of N,N,N',N",N"-pentamethyldiethylenetriamine (N,N,N',N",N"-pentamethyldiethylenetriamine), 0.07g of cuprous bromide, stir thoroughly at 70°C for 1h to obtain a cellulose-based polyethylene oxide polymer.
[0038] 0.2 g of 1-vinylimidazole was added to the above cellulose-based polyethylene oxide polymer system using a disposable syringe and stirred for 3 hours. Then, it was fully diluted with a large amount of 2-butanone and stirred for 48 hours, and then copper ions were removed by chromatography column, and washed with a large amount of ethanol solution to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer, which was vacuum dried for 24 hours.
[0039] The brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer was dissolved in DMF, and 15 wt% of lithium bis(trifluoromethanesulfonyl)imide was added, and stirred in a water bath at 50°C for 12 hours to obtain a clear solution. The solution was then evenly dripped onto a polytetrafluoroethylene paper with a diameter of about d=2.2 mm, and then cast into a polytetrafluoroethylene mold with a diameter of 20 mm, the solvent was evaporated, and vacuum dried at 60°C for 12 hours, and then transferred to a glove box for storage to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte.
[0040] LiFeO4 was used as the positive electrode material, Li sheet as the negative electrode material, and four-arm polyethylene oxide-polymerized ionic liquid block copolymer all-solid electrolyte as the separator. LIR2016 button cells were manufactured in a glove box and tested using the LAND battery test system at 0.5 mA cm -2 and 0.1 mA cm -2 The test was carried out by charging and discharging for 0.5h at a constant current density.
[0041] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer. The characteristic peaks of protons from the polyethylene oxide segment appear at 3.6ppm (peak d, -CH2-CH2-O-) and 3.3ppm (peak e, -O-CH3), and the characteristic peaks from 1-vinyl imidazole are mainly around 8.2ppm, further proving that the product is the target compound. In addition, the baseline in the figure is flat and there are no obvious impurity peaks, indicating that the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer has a correct structure and high purity. Figure 3 It can be seen that the glass transition temperature T of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer isg The temperature is about -45.7℃, and the chain segments have strong mobility. Figure 4 It can be obtained that the 60°C conductivity of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer electrolyte membrane is 1.2×10 -4 S cm -1 It can be seen from the figure that the logarithm of conductivity and the inverse of temperature show a good linear relationship, which conforms to the Arrhenius equation. Figure 5 The ion migration number of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer electrolyte membrane is 0.32. Figure 6 The electrochemical window of the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer electrolyte membrane is 5.3V, which is greater than 4.8V and meets the application requirements of conventional lithium batteries. Figure 7 It can be seen that the initial discharge capacity of the lithium metal battery assembled by the brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer electrolyte separator can reach 153 mAh g at a rate of 0.1C. -1 . Figure 8 To test the battery's cycle performance in a high current density environment of 0.5C, the initial capacity of the battery is 128mAh / g. After 100 cycles, its capacity level can be maintained at 112mAh / g. Fig. 9 The rate performance of the battery at current densities of 0.1C, 0.1C, 0.5C and 1C, the capacity can reach 153mAh / g, 148mAh / g, 128mAh / g and 121mAh / g respectively, and after high-rate cycling, the capacity of the battery can still be restored, indicating that the battery has excellent rate performance.
[0042] Example 2: (x is 120, y is 120, m is 120)
[0043] In a glove box filled with argon, weigh 2g of microcrystalline cellulose in a round-bottom flask, add 10g of ionic liquid and stir thoroughly, then add 20mL of DMF, the process needs to be added dropwise gradually, and step-wise cooling is adopted at the same time, and finally placed in an ice-water bath for 1h, then slowly add 2-bromoisobutyryl bromide 20g dropwise, then cool and finally place in an ice-water bath for 15min, finally stir at room temperature for 48h, after stirring, add a large amount of deionized water in the flask to obtain a white precipitate, and then dissolve the white product with acetone. Then recrystallize with ethanol and other reagents, repeat the washing operation 5 times, and finally dry in an oven at about 70-80℃ under vacuum to obtain a cellulose skeleton bromine initiator.
[0044] Take 0.2g of cellulose skeleton bromine initiator and add 10mL DMF, stir thoroughly for 1.5h, after the white solid is completely dissolved, add 0.2g of polyethylene glycol methacrylate -CH3, 0.14g of N,N,N',N",N"-pentamethyldiethylenetriamine (N,N,N',N",N"-pentamethyldiethylenetriamine), 0.07g of cuprous bromide, stir thoroughly at 70°C for 1h to obtain a cellulose-based polyethylene oxide polymer.
[0045] 0.2 g of 1-vinylimidazole was added to the above cellulose-based polyethylene oxide polymer system using a disposable syringe and stirred for 3 hours. Then, it was fully diluted with a large amount of 2-butanone and stirred for 48 hours, followed by removal of copper ions using a chromatography column, and washed with a large amount of ethanol solution to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer, which was vacuum dried for 24 hours.
[0046] The brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer was dissolved in DMF, 25wt% of lithium salt was added, and stirred in a 50°C water bath for 12 hours to obtain a clear solution. The solution was then evenly dripped onto a polytetrafluoroethylene paper with a diameter of about d = 2.2 mm, and then cast into a polytetrafluoroethylene mold with a diameter of 20 mm, the solvent was evaporated, and vacuum dried at 60°C for 12 hours, and then transferred to a glove box for storage to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte.
[0047] Example 3: (x is 200, y is 200, m is 200)
[0048] In a glove box filled with argon, weigh 2g of microcrystalline cellulose in a round-bottom flask, add 10g of ionic liquid and stir thoroughly, then add 20mL of DMF, the process needs to be added dropwise gradually, and step-wise cooling is adopted at the same time, and finally placed in an ice-water bath for 1h, then slowly add 2-bromoisobutyryl bromide 25g dropwise, then cool and finally place in an ice-water bath for 15min, finally stir at room temperature for 48h, after stirring, add a large amount of deionized water in the flask to obtain a white precipitate, and then dissolve the white product with acetone. Recrystallize with ethanol and other reagents, repeat the washing operation 5 times, and finally dry in an oven at about 70-80℃ under vacuum to obtain a cellulose skeleton bromine initiator.
[0049] Take 0.2g of cellulose skeleton bromine initiator and add 10mL DMF, stir thoroughly for 1.5h, after the white solid is completely dissolved, add 0.2g of polyethylene glycol methacrylate -CH3, 0.14g of N,N,N',N",N"-pentamethyldiethylenetriamine (N,N,N',N",N"-pentamethyldiethylenetriamine), 0.07g of cuprous bromide, stir thoroughly at 70°C for 1h to obtain a cellulose-based polyethylene oxide polymer.
[0050] 0.2 g of 1-vinylimidazole was added to the above cellulose-based polyethylene oxide polymer system using a disposable syringe and stirred for 3 hours. Then, it was fully diluted with a large amount of 2-butanone and stirred for 48 hours, followed by removal of copper ions using a chromatography column, and washed with a large amount of ethanol solution to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer, which was vacuum dried for 24 hours.
[0051] The brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer was dissolved in DMF, 20wt% of lithium salt was added, and stirred in a 50°C water bath for 12 hours to obtain a clear solution. The solution was then evenly dripped onto a polytetrafluoroethylene paper with a diameter of about d = 2.2 mm, and then cast into a polytetrafluoroethylene mold with a diameter of 20 mm, the solvent was evaporated, and vacuum dried at 60°C for 12 hours, and then transferred to a glove box for storage to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte.
[0052] Example 4: (x is 1500, y is 150, m is 150)
[0053] In a glove box filled with argon, weigh 2g of microcrystalline cellulose in a round-bottom flask, add 10g of ionic liquid and stir thoroughly, then add 20mL of DMF, the process needs to be added dropwise gradually, and the temperature is lowered stepwise, and finally placed in an ice-water bath for 1h, then slowly add 30g of 2-bromoisobutyryl bromide dropwise, then cool and finally place in an ice-water bath for 15min, finally stir at room temperature for 48h, after stirring, add a large amount of deionized water in the flask to obtain a white precipitate, and then dissolve the white product with acetone. Recrystallize with ethanol and other reagents, repeat the washing operation ~ 5 times, and finally dry in an oven at about 70-80℃ under vacuum to obtain a cellulose skeleton bromine initiator.
[0054] Take 0.2g of cellulose skeleton bromine initiator and add 10mL DMF, stir thoroughly for 1.5h, after the white solid is completely dissolved, add 0.2g of polyethylene glycol methacrylate -CH3, 0.14g of N,N,N',N",N"-pentamethyldiethylenetriamine (N,N,N',N",N"-pentamethyldiethylenetriamine), 0.07g of cuprous bromide, stir thoroughly at 70°C for 1h to obtain a cellulose-based polyethylene oxide polymer.
[0055] 0.2 g of 1-vinylimidazole was added to the above cellulose-based polyethylene oxide polymer system using a disposable syringe and stirred for 3 hours. Then, it was fully diluted with a large amount of 2-butanone and stirred for 48 hours, followed by removal of copper ions using a chromatography column, and washed with a large amount of ethanol solution to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer, which was vacuum dried for 24 hours.
[0056] The brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer was dissolved in DMF, 25wt% of lithium salt was added, and stirred in a 50°C water bath for 12 hours to obtain a clear solution. The solution was then evenly dripped onto a polytetrafluoroethylene paper with a diameter of about d = 2.2 mm, and then cast into a polytetrafluoroethylene mold with a diameter of 20 mm, the solvent was evaporated, and vacuum dried at 60°C for 12 hours, and then transferred to a glove box for storage to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte.
[0057] Example 5: (x is 150, y is 150, m is 150)
[0058] In a glove box filled with argon, weigh 2g of microcrystalline cellulose in a round-bottom flask, add 10g of ionic liquid and stir thoroughly, then add 20mL of DMF, the process needs to be added dropwise gradually, and step-wise cooling is adopted at the same time, and finally placed in an ice-water bath for 1h, then slowly add 2-bromoisobutyryl bromide 20g dropwise, then cool and finally place in an ice-water bath for 15min, finally stir at room temperature for 48h, after stirring, add a large amount of deionized water in the flask to obtain a white precipitate, and then dissolve the white product with acetone. Then recrystallize with ethanol and other reagents, repeat the washing operation ~ 5 times, and finally dry in an oven at about 70-80℃ under vacuum to obtain a cellulose skeleton bromine initiator.
[0059] Take 0.2g of cellulose skeleton bromine initiator and add 10mL DMF, stir thoroughly for 1.5h, after the white solid is completely dissolved, add 0.2g of polyethylene glycol methacrylate -CH3, 0.14g of N,N,N',N",N"-pentamethyldiethylenetriamine (N,N,N',N",N"-pentamethyldiethylenetriamine), 0.07g of cuprous bromide, stir thoroughly at 70°C for 1h to obtain a cellulose-based polyethylene oxide polymer.
[0060] 0.2 g of 1-vinylimidazole was added to the above cellulose-based polyethylene oxide polymer system using a disposable syringe and stirred for 3 hours. Then, it was fully diluted with a large amount of 2-butanone and stirred for 48 hours, followed by removal of copper ions using a chromatography column, and washed with a large amount of ethanol solution to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer, which was vacuum dried for 24 hours.
[0061] The brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer was dissolved in DMF, 25wt% of lithium salt was added, and stirred in a 50°C water bath for 12 hours to obtain a clear solution. The solution was then evenly dripped onto a polytetrafluoroethylene paper with a diameter of about d = 2.2 mm, and then cast into a polytetrafluoroethylene mold with a diameter of 20 mm, the solvent was evaporated, and vacuum dried at 60°C for 12 hours, and then transferred to a glove box for storage to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte.
[0062] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. Application of a block polymer based on a brush-like cellulose skeleton as a solid electrolyte, characterized in that: The preparation method of the block polymer based on the brush-like cellulose skeleton is: In a glove box filled with argon, weigh 2 g of microcrystalline cellulose, add 10 g of 1-allyl-3-methylimidazole chloride and stir thoroughly, add 20 mL of DMF dropwise, cool in a stepwise manner, and finally place in an ice water bath for 1 hour, then add 20 g of 2-bromoisobutyryl bromide dropwise, then cool, place in an ice water bath for 15 minutes, and finally stir at room temperature for 48 hours. After the stirring is completed, add deionized water to obtain a white precipitate, then dissolve the white precipitate with acetone, and then recrystallize with ethanol. The washing operation is repeated 5 times, and finally vacuum dried in an oven at 70-80°C to obtain a cellulose skeleton bromine initiator; Take 0.2g of cellulose skeleton bromine initiator and add 10mL of DMF, stir thoroughly for 1.5h, after the white solid is completely dissolved, add 0.2g of polyethylene glycol methacrylate -CH3, 0.14g of N,N,N′,N″,N″-pentamethyldiethylenetriamine, and 0.07g of cuprous bromide, stir thoroughly at 70°C for 1h to obtain a cellulose-based polyethylene oxide polymer; 0.2 g of 1-vinylimidazole was added to the cellulose-based polyethylene oxide polymer, stirred for 3 h, then fully diluted with 2-butanone and stirred for 48 h, then the copper ions were removed by chromatography column, washed with ethanol solution to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer, and vacuum dried for 24 h; The brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer is dissolved in DMF, 15 wt % of lithium bis(trifluoromethanesulfonyl)imide is added, and the mixture is stirred in a water bath at 50° C. for 12 h to obtain a clear solution, and then the clear solution is evenly dropped onto a polytetrafluoroethylene paper with a diameter of 2.2 mm, and then cast into a polytetrafluoroethylene mold with a diameter of 20 mm, the solvent is evaporated, and the mixture is vacuum dried at 60° C. for 12 h, and then transferred to a glove box for storage to obtain a brush-like cellulose-based polyethylene oxide-polyvinyl imidazole block copolymer solid electrolyte; The main chain skeleton of the block polymer is cellulose, and the side chain is composed of polyethylene oxide and polyvinyl imidazole block copolymers. The general structural formula is shown below: Among them, x is 60-280, y is 80, m is 100, and n is 220.