Metal silicide layer and method for preparing semiconductor structure

By depositing a metal layer on the surface of the silicon substrate to form a transition metal silicide layer and performing an annealing treatment, the problem of cumbersome traditional processes is solved, and the effect of simplifying the process flow and improving the preparation efficiency is achieved.

CN115332063BActive Publication Date: 2024-11-12HEFEI XINJING INTEGRATED CIRCUIT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210972332.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-15
Publication Date
2024-11-12
Estimated Expiration
2042-08-15

AI Technical Summary

Technical Problem

The process of preparing traditional metal silicides is cumbersome, requiring multiple annealing processes and covering layers, resulting in complexity in the process.

Method used

A metal layer is deposited on the surface of the silicon substrate and a transition metal silicide layer is formed, which is converted into a metal silicide layer through a one-time annealing treatment, simplifying the process flow and avoiding the formation of a cover layer.

Benefits of technology

The preparation process of the metal silicide layer is simplified, the process steps and time are reduced, and the preparation efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115332063B_ABST
    Figure CN115332063B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a metal silicide layer and a semiconductor structure. The method for preparing a metal silicide layer comprises: providing a silicon substrate; depositing a metal layer on the surface of the silicon substrate at a preset deposition temperature, during which part of the metal layer reacts with part of the silicon substrate to form a transition metal silicide layer of a metal-rich phase; the transition metal silicide layer is located between the unreacted metal layer and the unreacted silicon substrate; and annealing the silicon substrate with the transition metal silicide layer formed on the surface to convert the transition metal silicide layer into a metal silicide layer. The present application can simplify the process flow.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of integrated circuit technology, and in particular to a method for preparing a metal silicide layer and a semiconductor structure. Background Art

[0002] With the development of integrated circuit technology, metal silicides are widely used in contact layers in semiconductor structures to reduce contact resistance due to their low resistivity. In the traditional process flow of preparing metal silicides, it is usually necessary to first deposit certain metals (such as nickel) on a silicon (Si) substrate, and form a covering layer (such as titanium nitride) on the metal surface to prevent metal oxidation. Finally, multiple annealing processes are required to form metal silicides as contact layers in semiconductor structures, which has the problem of a relatively cumbersome process flow. Summary of the invention

[0003] Based on this, it is necessary to provide a method for preparing a metal silicide layer and a semiconductor structure to address the problem of complicated process flow in traditional technologies.

[0004] In order to achieve the above object, on the one hand, the present invention provides a method for preparing a metal silicide layer, the method for preparing a metal silicide layer comprising:

[0005] providing a silicon substrate;

[0006] Depositing a metal layer on the surface of the silicon substrate at a preset deposition temperature, wherein a portion of the metal layer reacts with a portion of the silicon substrate during the deposition process to form a transition metal silicide layer of a metal-rich phase; the transition metal silicide layer is located between the unreacted metal layer and the unreacted silicon substrate;

[0007] The silicon substrate with the transition metal silicide layer formed on the surface is subjected to annealing treatment to transform the transition metal silicide layer into a metal silicide layer.

[0008] In one embodiment, the transition metal silicide layer includes: a first metal silicide layer and a second metal silicide layer, the first metal silicide layer is located on the unreacted upper surface of the silicon substrate; the second metal silicide layer is located between the first metal silicide layer and the unreacted metal layer.

[0009] In one embodiment, annealing the silicon substrate having the transition metal silicide layer formed on the surface thereof to convert the transition metal silicide layer into a metal silicide layer comprises:

[0010] The silicon substrate having the transition metal silicide layer formed on the surface is annealed to transform the second metal silicide layer into a first metal silicide layer; the first metal silicide layer formed during the annealing process and the first metal silicide layer formed during the deposition process together constitute the metal silicide layer.

[0011] In one embodiment, the metal layer includes a platinum-doped nickel layer.

[0012] In one of the embodiments, the molar concentration of platinum in the metal layer is 5% to 10%.

[0013] In one of the embodiments, the preset deposition temperature is 60°C to 180°C.

[0014] In one embodiment, before annealing the silicon substrate having the transition metal silicide layer formed on the surface, the method further comprises:

[0015] The unreacted metal layer is removed.

[0016] The method for preparing the metal silicide layer comprises: providing a silicon substrate; depositing a metal layer on the surface of the silicon substrate at a preset deposition temperature, during which part of the metal layer reacts with part of the silicon substrate to form a transition metal silicide layer rich in metal phase; the transition metal silicide layer is located between the unreacted metal layer and the unreacted silicon substrate; and annealing the silicon substrate with the transition metal silicide layer formed on the surface to convert the transition metal silicide layer into a metal silicide layer. Since the present invention does not need to form a covering layer during the preparation process, and only needs to undergo one annealing process to prepare the metal silicide layer, the process flow can be simplified.

[0017] The present invention also provides a method for preparing a semiconductor structure, the method for preparing a semiconductor structure comprising:

[0018] providing a substrate, wherein the substrate comprises a silicon substrate;

[0019] forming a gate structure on the surface of the substrate, wherein the gate structure comprises a polysilicon gate;

[0020] forming a source region and a drain region in the substrate, wherein the source region and the drain region are located on two opposite sides of the gate structure;

[0021] The metal silicide layer is formed on the surface of the polysilicon gate, the surface of the source region, and the surface of the drain region by using the method for preparing the metal silicide layer as described in any of the above embodiments.

[0022] In one embodiment, forming a gate structure on the surface of the substrate includes:

[0023] forming an oxide layer on the surface of the substrate;

[0024] forming a polysilicon layer on the surface of the oxide layer;

[0025] Etching the polysilicon layer and the oxide layer to form a stacked structure including a gate oxide layer and a polysilicon gate;

[0026] A sidewall is formed on the sidewall of the stacked structure.

[0027] In one embodiment, after forming a sidewall on the sidewall of the stacked structure, the method further comprises:

[0028] forming an etch stop layer on the surface of the substrate, the surface of the metal silicide layer and the surface of the sidewall;

[0029] forming an interlayer dielectric layer on the surface of the etch stop layer;

[0030] A contact hole is formed in the interlayer dielectric layer by etching.

[0031] The method for preparing the semiconductor structure includes: providing a substrate, the substrate including a silicon substrate; forming a gate structure on the surface of the substrate, the gate structure including a polysilicon gate; forming a source region and a drain region in the substrate, the source region and the drain region being located on opposite sides of the gate structure; and forming a metal silicide layer on the surface of the polysilicon gate, the surface of the source region, and the surface of the drain region using the method for preparing a metal silicide layer as in any of the above embodiments. Since the present invention does not need to form a covering layer during the preparation process, and only needs to undergo one annealing process to prepare the metal silicide layer, the process flow can be simplified. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0033] Figure 1 is a schematic flow chart of a method for preparing a metal silicide layer provided in an embodiment;

[0034] Figure 2 is a schematic cross-sectional view of a structure obtained in step S101 in a method for preparing a metal silicide layer provided in an embodiment;

[0035] Figure 3 is a schematic cross-sectional view of a structure obtained in step S102 in a method for preparing a metal silicide layer provided in an embodiment;

[0036] Figure 4 is a schematic cross-sectional view of a structure obtained in step S103 in a method for preparing a metal silicide layer provided in an embodiment;

[0037] Figure 5 A schematic cross-sectional view of the structure of a first metal silicide layer and a second metal silicide layer included in a transition metal silicide layer in a method for preparing a metal silicide layer provided in an embodiment;

[0038] Figure 6 is a schematic cross-sectional view of a structure obtained in step S103 in a method for preparing a metal silicide layer provided in another embodiment;

[0039] Figure 7 is a schematic cross-sectional view of a structure obtained after removing an unreacted metal layer in a method for preparing a metal silicide layer provided in another embodiment;

[0040] Figure 8 is a schematic flow chart of a method for preparing a semiconductor structure provided in an embodiment;

[0041] Fig. 9 is a schematic cross-sectional view of a structure obtained in step S801 in a method for preparing a semiconductor structure provided in an embodiment;

[0042] Fig.10 is a schematic cross-sectional view of a structure obtained in step S802 in a method for preparing a semiconductor structure provided in an embodiment;

[0043] Fig.11 is a schematic cross-sectional view of a structure obtained in step S803 in a method for preparing a semiconductor structure provided in an embodiment;

[0044] Fig.12 is a schematic cross-sectional view of a structure obtained in step S804 in a method for preparing a semiconductor structure provided in an embodiment;

[0045] Fig.13 It is a schematic diagram of a process of forming a gate structure on a surface of a substrate in a method for preparing a semiconductor structure provided in an embodiment;

[0046] Fig.14 is a schematic cross-sectional view of a structure obtained in step S1301 in a method for preparing a semiconductor structure provided in an embodiment;

[0047] Fig.15 is a schematic cross-sectional view of a structure obtained in step S1302 in a method for preparing a semiconductor structure provided in an embodiment;

[0048] Fig.16 is a schematic cross-sectional view of a structure obtained in step S1303 in a method for preparing a semiconductor structure provided in an embodiment;

[0049] Fig.17 is a schematic cross-sectional view of a structure obtained in step S1304 in a method for preparing a semiconductor structure provided in an embodiment;

[0050] Fig.18 It is a schematic diagram of the process after forming a sidewall spacer on the sidewall of the stacked structure in the method for preparing a semiconductor structure provided in one embodiment;

[0051] Fig.19 is a schematic cross-sectional view of a structure obtained in step S1801 in a method for preparing a semiconductor structure provided in an embodiment;

[0052] Fig. 20 is a schematic cross-sectional view of a structure obtained in step S1802 in a method for preparing a semiconductor structure provided in an embodiment;

[0053] Fig.21 It is a schematic cross-sectional view of a structure obtained in step S1803 in a method for preparing a semiconductor structure provided in one embodiment.

[0054] Description of reference numerals:

[0055] 10-silicon substrate, 20-metal layer, 30-transition metal silicide layer, 301-first metal silicide layer, 302-second metal silicide layer, 40-metal silicide layer, 50-gate structure, 501-oxide layer, 502-polysilicon layer, 60-source region, 70-drain region, 80-side wall, 90-etching stop layer, 901-interlayer dielectric layer, 902-contact hole. DETAILED DESCRIPTION

[0056] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. Embodiments of the present application are provided in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.

[0057] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0058] It should be understood that when an element or layer is referred to as being "on, adjacent to, connected to or coupled to other elements or layers, it may be directly on, adjacent to, connected to or coupled to other elements or layers, or there may be intervening elements or layers. On the contrary, when an element is referred to as being "directly on, directly adjacent to, directly connected to or directly coupled to other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, doping types and / or parts, these elements, components, regions, layers, doping types and / or parts should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, doping type or part from another element, component, region, layer, doping type or part. Therefore, without departing from the teachings of the present invention, the first element, component, region, layer, doping type or portion discussed below may be represented as a second element, component, region, layer or portion; for example, the first doping type may be referred to as the second doping type, and similarly, the second doping type may be referred to as the first doping type; the first doping type and the second doping type are different doping types, for example, the first doping type may be P-type and the second doping type may be N-type, or the first doping type may be N-type and the second doping type may be P-type.

[0059] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that, in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "above" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.

[0060] When used herein, the singular forms "a", "an" and " / the" may also include the plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "include / comprise" or "have" and the like specify the presence of stated features, wholes, steps, operations, components, parts or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, wholes, steps, operations, components, parts or combinations thereof. At the same time, in this specification, the term "and / or" includes any and all combinations of the relevant listed items.

[0061] Embodiments of the invention are described herein with reference to cross-sectional views which are schematic diagrams of ideal embodiments (and intermediate structures) of the invention, such that variations in the shapes shown due to, for example, manufacturing techniques and / or tolerances are anticipated. Thus, embodiments of the invention should not be limited to the specific shapes of the regions shown herein, but rather include deviations in shapes due to, for example, manufacturing techniques. For example, an implanted region shown as a rectangle typically has rounded or curved features and / or an implant concentration gradient at its edges rather than a binary change from an implanted region to a non-implanted region. Similarly, a buried region formed by implantation may result in some implantation in the region between the buried region and the surface through which the implantation is performed. Thus, the regions shown in the figures are schematic in nature, their shapes do not represent the actual shape of the region of the device, and do not limit the scope of the invention.

[0062] See also Figure 1 The present invention provides a method for preparing a metal silicide layer, comprising:

[0063] S101: providing a silicon substrate;

[0064] S102: depositing a metal layer on the surface of the silicon substrate at a preset deposition temperature, wherein a portion of the metal layer reacts with a portion of the silicon substrate to form a transition metal silicide layer of a metal-rich phase; the transition metal silicide layer is located between the unreacted metal layer and the unreacted silicon substrate;

[0065] S103: performing annealing treatment on the silicon substrate having the transition metal silicide layer formed on the surface thereof, so as to transform the transition metal silicide layer into a metal silicide layer.

[0066] The method for preparing a metal silicide layer of the present invention comprises: providing a silicon substrate; depositing a metal layer on the surface of the silicon substrate at a preset deposition temperature, during which part of the metal layer reacts with part of the silicon substrate to form a transition metal silicide layer of a metal-rich phase; the transition metal silicide layer is located between the unreacted metal layer and the unreacted silicon substrate; and annealing the silicon substrate with the transition metal silicide layer formed on the surface to convert the transition metal silicide layer into a metal silicide layer. Since the present invention does not need to form a covering layer during the preparation process, and only needs to undergo one annealing process to prepare the metal silicide layer, the process flow can be simplified.

[0067] In step S101, refer to Figure 1 Step S101 and Figure 2 , a silicon substrate 10 is provided.

[0068] In step S102, refer to Figure 1 Step S102 and Figure 3A metal layer 20 is deposited on the surface of a silicon substrate 10 at a preset deposition temperature. During the deposition process, a portion of the metal layer 20 reacts with a portion of the silicon substrate 10 to form a transition metal silicide layer 30 of a metal-rich phase; the transition metal silicide layer 30 is located between the unreacted metal layer 20 and the unreacted silicon substrate 10.

[0069] The material of the metal layer 20 may be one of metals such as tungsten (W), cobalt (Co), nickel (Ni), platinum (Pt) or titanium (Ti), or an alloy formed by multiple metals among the above metals, which is not limited in this embodiment.

[0070] Optionally, taking the metal layer 20 as an example of a material of nickel, the material of the metal-rich transition metal silicide layer 30 may be Ni x Si, where x ≥ 1.

[0071] Optionally, the deposition process of depositing the metal layer 20 on the surface of the silicon substrate 10 at a preset deposition temperature can be a physical vapor deposition (PVD) process, a chemical vapor deposition (CVD) process or an atomic layer deposition (ALD) process.

[0072] Preferably, the deposition process for depositing the metal layer 20 on the surface of the silicon substrate 10 at a preset deposition temperature is a PVD process.

[0073] In step S103, refer to Figure 1 Step S103 and Figure 4 The silicon substrate 10 having the transition metal silicide layer 30 formed on the surface thereof is annealed to transform the transition metal silicide layer 30 into the metal silicide layer 40 .

[0074] Optionally, taking the case where the material of the metal layer 20 is nickel as an example, the material of the metal silicide layer 40 may be NiSi.

[0075] Optionally, taking the material of the metal layer 20 as nickel as an example, the temperature of the annealing treatment may be 400° C. to 800° C.

[0076] In one embodiment, see Figure 5 The transition metal silicide layer 30 includes: a first metal silicide layer 301 and a second metal silicide layer 302 , the first metal silicide layer 301 is located on the upper surface of the unreacted silicon substrate 10 ; the second metal silicide layer 302 is located between the first metal silicide layer 301 and the unreacted metal layer 20 .

[0077] Optionally, taking the metal layer 20 as an example, the material of the first metal silicide layer 301 may be NiSi, and the material of the second metal silicide layer 302 may be Ni. x Si, where x ≥ 2.

[0078] In one embodiment, see Figure 6 The above step S103 includes: annealing the silicon substrate 10 with the transition metal silicide layer 30 formed on the surface to transform the second metal silicide layer 302 into the first metal silicide layer 301; the first metal silicide layer 301 formed during the annealing process and the first metal silicide layer 301 formed during the deposition process together constitute a metal silicide layer 40.

[0079] In one embodiment, metal layer 20 includes a platinum-doped nickel layer.

[0080] Optionally, taking the deposition process as a PVD process and the material of the metal layer 20 as metal nickel as an example, a certain molar concentration of metal platinum can be doped into the metal nickel in the PVD process so that the formed metal layer 20 is a platinum-doped nickel layer. The platinum-doped nickel layer has good high-temperature stability, can improve the interface morphology, and reduce defects.

[0081] In one embodiment, the molar concentration of platinum in the metal layer 20 is 5% to 10%.

[0082] In one embodiment, the preset deposition temperature is 60°C to 180°C.

[0083] Optionally, the preset deposition temperature may also be higher than room temperature, so that the metal layer 20 reacts with the silicon substrate 10 during the deposition process to form a transition metal silicide layer 30 .

[0084] In one embodiment, see Figure 7 Before annealing the silicon substrate 10 having the transition metal silicide layer 30 formed on the surface thereof, the method further includes: removing the unreacted metal layer 20 .

[0085] See also Figure 8 The present invention also provides a method for preparing a semiconductor structure, characterized in that the method for preparing a semiconductor structure comprises:

[0086] S801: providing a substrate, wherein the substrate includes a silicon substrate;

[0087] S802: forming a gate structure on a surface of the substrate, the gate structure comprising a polysilicon gate;

[0088] S803: forming a source region and a drain region in the substrate, wherein the source region and the drain region are located on two opposite sides of the gate structure;

[0089] S804: Forming a metal silicide layer on the surface of the polysilicon gate, the surface of the source region, and the surface of the drain region by using the method for preparing a metal silicide layer as described in any of the above embodiments.

[0090] The method for preparing a semiconductor structure of the present invention comprises: providing a substrate, the substrate comprising a silicon substrate; forming a gate structure on the surface of the substrate, the gate structure comprising a polysilicon gate; forming a source region and a drain region in the substrate, the source region and the drain region being located on opposite sides of the gate structure; and forming a metal silicide layer on the surface of the polysilicon gate, the surface of the source region, and the surface of the drain region using the method for preparing a metal silicide layer as in any of the above embodiments. Since the present invention does not need to form a covering layer during the preparation process, and only needs to undergo one annealing process to prepare the metal silicide layer, the process flow can be simplified.

[0091] In step S801, refer to Figure 8 Step S801 and Fig. 9 , a substrate is provided, the substrate comprising a silicon substrate 10.

[0092] Optionally, the substrate may also include a silicon carbide substrate, a sapphire substrate, etc., and a suitable substrate may be selected according to the actual application scenario.

[0093] In step S802, refer to Figure 8 Step S802 and Fig.10 , a gate structure 50 is formed on the surface of the substrate, and the gate structure 50 includes a polysilicon gate.

[0094] In step S803, refer to Figure 8 Step S803 and Fig.11 , a source region 60 and a drain region 70 are formed in the substrate, and the source region 60 and the drain region 70 are located on two opposite sides of the gate structure 50 .

[0095] In step S804, refer to Figure 8 Step S804 and Fig.12 A metal silicide layer 40 is formed on the surface of the polysilicon gate, the surface of the source region 60 and the surface of the drain region 70 using the method for preparing the metal silicide layer 40 as described in any of the above embodiments.

[0096] In one embodiment, see Fig.13 , forming a gate structure on the surface of the substrate, including:

[0097] S1301: forming an oxide layer on the surface of the substrate;

[0098] S1302: forming a polysilicon layer on the surface of the oxide layer;

[0099] S1303: etching the polysilicon layer and the oxide layer to form a stacked structure including a gate oxide layer and a polysilicon gate;

[0100] S1304: forming a sidewall on the sidewall of the stacked structure.

[0101] In step S1301, refer to Fig.13 Step S1301 and Fig.14 , an oxide layer 501 is formed on the surface of the substrate.

[0102] In step S1302, refer to Fig.13 Step S1302 and Fig.15 , a polysilicon layer 502 is formed on the surface of the oxide layer 501.

[0103] In step S1303, refer to Fig.13 Step S1303 and Fig.16 , the polysilicon layer 502 and the oxide layer 501 are etched to form a stacked structure including the gate oxide layer 501 and the polysilicon gate.

[0104] In step S1304, refer to Fig.13 Step S1304 and Fig.17 , forming a sidewall 80 on the sidewall of the stacked structure.

[0105] The sidewall 80 may be formed by etching. Optionally, the sidewall may be made of one or more of silicon oxide, silicon nitride, silicon oxynitride, and silicon carbide, which is not limited in this embodiment.

[0106] In one embodiment, see Fig.18 , after forming a side wall on the side wall of the stacked structure, further comprising:

[0107] S1801: forming an etching stop layer on the surface of the substrate, the surface of the metal silicide layer, and the surface of the sidewall;

[0108] S1802: forming an interlayer dielectric layer on the surface of the etch stop layer;

[0109] S1803: forming contact holes in the interlayer dielectric layer by etching.

[0110] In step S1801, refer to Fig.18 Step S1801 and Fig.19 An etch stop layer 90 is formed on the surface of the substrate, the surface of the metal silicide layer 40 and the surface of the sidewall spacer 80 .

[0111] Optionally, the material of the etch stop layer 90 may be one or more of silicon carbide, silicon nitride, and silicon oxynitride, which is not limited in this embodiment.

[0112] In step S1802, refer to Fig.18 Step S1802 and Fig. 20 , an interlayer dielectric layer 901 is formed on the surface of the etch stop layer 90 .

[0113] Optionally, the interlayer dielectric layer 901 may be manufactured by a high-density plasma chemical vapor deposition process.

[0114] Optionally, the material of the interlayer dielectric layer 901 may be silicon oxide or borophosphosilicate glass, etc., which is not limited in this embodiment.

[0115] In step S1803, refer to Fig.18 Step S1803 and Fig.21 , a contact hole 902 is formed in the interlayer dielectric layer 901 by etching.

[0116] Optionally, before the above step S1803, the process may further include: using a chemical mechanical polishing (CMP) process to planarize the surface of the interlayer dielectric layer 901.

[0117] Optionally, the etching process for forming the contact hole 902 may include reactive ion etching (RIE) or plasma etching, etc., which is not limited in this embodiment.

[0118] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features of the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0119] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for preparing a metal silicide layer, characterized in that: The method for preparing the metal silicide layer comprises: providing a silicon substrate; A metal layer is deposited on the surface of the silicon substrate at a preset deposition temperature, during which a portion of the metal layer reacts with a portion of the silicon substrate to form a transition metal silicide layer of a metal-rich phase; the transition metal silicide layer is located between the unreacted metal layer and the unreacted silicon substrate; the transition metal silicide layer includes a first metal silicide layer and a second metal silicide layer, the first metal silicide layer is located on the upper surface of the unreacted silicon substrate; the second metal silicide layer is located between the first metal silicide layer and the unreacted metal layer; The silicon substrate with the transition metal silicide layer formed on the surface is annealed to transform the second metal silicide layer into a first metal silicide layer; the first metal silicide layer formed during the annealing process and the first metal silicide layer formed during the deposition process together constitute a metal silicide layer.

2. The method for preparing a metal silicide layer according to claim 1, characterized in that: The metal layer includes a platinum-doped nickel layer.

3. The method for preparing a metal silicide layer according to claim 2, characterized in that: In the metal layer, the molar concentration of platinum is 5% to 10%.

4. The method for preparing a metal silicide layer according to claim 1, characterized in that: The preset deposition temperature is 60°C to 180°C.

5. The method for preparing a metal silicide layer according to claim 1, characterized in that: Before annealing the silicon substrate having the transition metal silicide layer formed on the surface thereof, the method further comprises: The unreacted metal layer is removed.

6. The method for preparing a metal silicide layer according to claim 1, characterized in that: The material of the first metal silicide layer is NiSi, and the material of the second metal silicide layer is Ni x Si, where x≥2.

7. The method for preparing a metal silicide layer according to claim 1, characterized in that: The annealing treatment is performed at a temperature of 400°C to 800°C.

8. A method for preparing a semiconductor structure, characterized in that: The method for preparing the semiconductor structure comprises: providing a substrate, wherein the substrate comprises a silicon substrate; forming a gate structure on the surface of the substrate, wherein the gate structure comprises a polysilicon gate; forming a source region and a drain region in the substrate, wherein the source region and the drain region are located on two opposite sides of the gate structure; The metal silicide layer is formed on the surface of the polysilicon gate, the surface of the source region and the surface of the drain region by using the method for preparing the metal silicide layer according to any one of claims 1 to 7.

9. The method for preparing a semiconductor structure according to claim 8, characterized in that: The forming of a gate structure on the surface of the substrate comprises: forming an oxide layer on the surface of the substrate; forming a polysilicon layer on the surface of the oxide layer; Etching the polysilicon layer and the oxide layer to form a stacked structure including a gate oxide layer and a polysilicon gate; A sidewall is formed on the sidewall of the stacked structure.

10. The method for preparing a semiconductor structure according to claim 9, characterized in that: After forming a sidewall on the sidewall of the stacked structure, the method further comprises: forming an etching stop layer on the surface of the substrate, the surface of the metal silicide layer and the surface of the sidewall; forming an interlayer dielectric layer on the surface of the etch stop layer; A contact hole is formed in the interlayer dielectric layer by etching.