A supported magnesium oxide dechlorinating agent and its preparation method and application
Through the preparation of γ-Al2O3-loaded magnesium oxide dehydration agent, the problem of inefficient dehydration in the prior art was solved, and the efficient and low-temperature flue gas dechlorination effect was achieved, and the dechlorination performance of coal-fired power plants was improved.
Patent Information
- Application Number
- CN202211145636.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-09-20
AI Technical Summary
The existing coal-fired flue gas dechlorination agent has low dechlorination efficiency at 150-200°C, which cannot meet the needs of coal-fired power plants. Dechlorination agents such as sodium bicarbonate and alkaline earth metal have poor dehydration effect within this temperature range.
Using γ-Al2O3-supported magnesium oxide dechlorination agent, a dechlorination agent with a high specific surface area and a developed pore structure is prepared by mixing water, magnesium salt and γ-Al2O3 in a specific proportion, and stirring, drying, calcining and grinding to form a dechlorination agent with a high specific surface area and a developed pore structure to improve the dechlorination efficiency.
The dechlorination efficiency and low-temperature dechlorination effect are significantly improved, and the HCl in flue gas is efficiently removed at 150-200℃, the desulfurization wastewater volume and Cl- content in gypsum are reduced, and the quality of gypsum is improved.
Smart Images

Figure CN115350576B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coal-fired flue gas dechlorination, in particular to a supported magnesium oxide dechlorination agent and a preparation method and application thereof. Background Art
[0002] Thermal power plants use a large amount of coal and other fossil fuels. During the coal combustion process, more than 90% of the chlorine in the coal volatilizes into the flue gas in the form of hydrogen chloride. If the chlorine-containing gas in the flue gas is discharged into the atmosphere, it will cause an increase in acid rain and cause great harm to nature and humans. In addition, because it is highly acidic, it will cause corrosion on the heating surface of the pipe in the combustion system, thereby seriously shortening the service life of the equipment.
[0003] Since the HCl content in coal-fired flue gas is relatively low, there is no separate dechlorination measure for flue gas treatment in power plants at present. Instead, most of the chloride ions in the flue gas are enriched in the desulfurization tower through the wet desulfurization system. More than 92% of the chloride ions in the wet desulfurization device come from coal-fired flue gas. The chlorine in the flue gas is absorbed and enriched in the desulfurization slurry, resulting in Cl in the desulfurization slurry. - The content continues to increase, and when it exceeds a certain concentration, it needs to be discharged regularly to form desulfurization wastewater. Therefore, the increase in the chloride ion concentration in the desulfurization slurry will not only reduce the utilization rate of the desulfurizer and the desulfurization efficiency, causing corrosion of the equipment, but also seriously reduce the quality of the desulfurization by-product gypsum, and will also affect the safe and stable operation of the desulfurization device.
[0004] Flue gas dechlorination is a technical solution that removes HCl from the source and reduces the chloride concentration entering the desulfurization tower, thereby reducing the amount of desulfurization wastewater and improving the quality of desulfurization gypsum. Flue gas dechlorination is to inject a high-efficiency dechlorinating agent into the flue, fully mix it with the flue gas, and react with acid and alkali to remove hydrogen chloride. The reaction product, chloride salt, is removed by a dust removal device, thereby greatly reducing the Cl entering the desulfurization tower. - concentration, reducing the amount of desulfurization wastewater and lowering the Cl - content, thus improving the quality of gypsum.
[0005] Therefore, compared with the dechlorination technology of desulfurization wastewater, the flue gas dechlorination technology has a simple system, low cost, high dechlorination efficiency, small footprint, no waste liquid generation, small flue gas temperature drop, and the dechlorination agent after dechlorination does not affect the quality of fly ash, which can achieve the reduction of desulfurization wastewater.
[0006] However, the dechlorination agents currently used generally have the following problems: 1. The dechlorination efficiency of ordinary calcium-based dechlorination agents at 150-200°C is very low and cannot meet the dechlorination efficiency required for flue gas injection dechlorination in coal-fired power plants; 2. Dechlorination agents such as sodium bicarbonate and alkaline earth metals require a certain activation temperature and have poor dechlorination effects in the range of 150-200°C.
[0007] In view of this, the present invention is proposed. Summary of the invention
[0008] The object of the present invention is to provide a supported magnesium oxide dechlorinating agent and a preparation method and application thereof. The γ-Al2O3 supported magnesium oxide dechlorinating agent has the advantages of high dechlorination efficiency, good low-temperature dechlorination effect and the like.
[0009] The present invention provides a method for preparing a supported magnesium oxide dechlorinating agent, comprising the following steps:
[0010] Mixing water, magnesium salt and γ-Al2O3 to obtain a mixed solution, stirring, drying, calcining and grinding the obtained mixed solution in sequence to obtain the supported magnesium oxide dechlorination agent;
[0011] Wherein, the mass ratio of water, magnesium salt and γ-Al2O3 is 200:(3.2-19.2):10.
[0012] The study found that after being loaded with γ-Al2O3, the dechlorination effect and low-temperature dechlorination effect of the magnesium-based dechlorinating agent were significantly improved. The reason may be: γ-Al2O3 is used to activate magnesium salts, and the γ-Al2O3 skeleton can play the role of supporting active components in the dechlorinating agent, providing a porous and loose environment for MgO, thereby increasing the mass transfer rate of gas inside the dechlorinating agent and exposing more active sites of magnesium oxide.
[0013] The present invention does not strictly limit the mass ratio of water, magnesium salt and γ-Al2O3. However, in order to ensure a better dechlorination effect, the mass ratio of water, magnesium salt and γ-Al2O3 can be controlled to be 200:(3.2-19.2):10. That is, under normal circumstances, as the Mg content increases, the dechlorination efficiency of the dechlorinator increases. However, when the Mg content increases to a certain level, its dechlorination efficiency decreases instead. This may be because, on the one hand, the pores between the Al2O3 skeletons will be blocked by the active components, and the gas diffusion in the dechlorinator encounters greater resistance. On the other hand, the active sites of the dechlorinator are blocked with each other and cannot contact HCl, so that the number of active sites is reduced, thereby reducing the dechlorination efficiency.
[0014] Specifically, the magnesium salt used in the present invention is Mg(NO3)2·6H2O or Mg(CH3COO)2·4H2O, which is used as the dechlorination agent matrix. Under the specific reaction conditions, the precursor of the magnesium salt can effectively form magnesium oxide crystals, and at the same time, it will not cause a large amount of agglomeration of the product due to excessive temperature.
[0015] The present invention does not impose strict restrictions on the specific conditions of stirring, as long as the magnesium salt precursor and γ-Al2O3 are fully mixed, the magnesium salt is evenly distributed on the skeleton of γ-Al2O3, and a richer pore structure is provided for MgO, thereby increasing the mass transfer rate of the gas inside the dechlorinating agent, and exposing more active sites of MgO. Specifically, during the stirring, magnetic stirring is performed in a water bath at 55-65°C for 2-12 hours until the mixture is semi-dry.
[0016] The present invention does not impose strict restrictions on the specific conditions of drying. In one embodiment, during drying, a blast drying oven is used, and the temperature is controlled to be 100-110° C. for 10-20 hours to obtain a dry block solid to ensure the integrity of the void structure of the dechlorination agent.
[0017] The present invention does not impose strict restrictions on the specific conditions of calcination. Specifically, during calcination, the dried block solid is placed on a ceramic ark, and the temperature is controlled at 500-510° C. in a muffle furnace under a nitrogen atmosphere, and calcined for 3-5 hours to obtain a block solid. Under the specific calcination conditions, the precursor of the magnesium salt can effectively form magnesium oxide crystals, and at the same time, the product will not agglomerate in large quantities due to excessively high temperatures.
[0018] Finally, the calcined block solid is ground in a mortar, and after grinding, it is passed through a 20-40 mesh sieve to obtain a γ-Al2O3-loaded magnesium oxide dechlorination agent. Specifically, the BET specific surface area of the γ-Al2O3-loaded magnesium oxide dechlorination agent is 180-215 m 2 / g, pore volume is 0.30-0.55cm 3 / g, pore size is 10-10.5nm.
[0019] The γ-Al2O3-loaded magnesium oxide dechlorinating agent prepared by the above method should also belong to the protection scope of the present invention, and studies have shown that the removal rate of HCl by the γ-Al2O3-loaded magnesium oxide dechlorinating agent of the present invention is 50-75% within 5 minutes.
[0020] The present invention also provides the application of the above-mentioned γ-Al2O3 loaded magnesium oxide dechlorinating agent in the dechlorination technology of coal-fired flue gas.
[0021] The present invention also provides a flue gas dechlorination method, which uses the above-mentioned γ-Al2O3-loaded magnesium oxide dechlorinating agent to dechlorinate the flue gas; wherein the temperature during dechlorination is 150-200° C. Its excellent low-temperature dechlorination effect is due to: on the one hand, magnesium oxide is a typical alkali metal oxide, and its frontier orbital easily gives electrons, which is conducive to bonding with acid and realizing acid-base reaction; on the other hand, γ-Al2O3 provides a good dechlorinating agent carrier, has a good pore structure, can disperse magnesium oxide, and is conducive to dechlorination.
[0022] The γ-Al2O3-loaded magnesium oxide dechlorinating agent of the present invention has at least the following technical effects:
[0023] 1. The preparation method of the γ-Al2O3-loaded magnesium oxide dechlorinating agent of the present invention is simple, the production and operation cost is low, the economy is good, and it is easy to mass produce and industrialize;
[0024] 2. The γ-Al2O3-loaded magnesium oxide dechlorinating agent of the present invention has strong chemical activity, developed pores, and a large specific surface area. When it is used in the coal-fired flue gas jet dechlorination technology, it has an excellent low-temperature dechlorination effect at 150-200°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 This is a SEM photo of the dechlorinating agent obtained in Example 1 of the present invention;
[0027] Figure 2 This is a SEM photograph of the dechlorinating agent obtained in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0028] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0029] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] S1. Mix water, Mg(NO3)2·6H2O and γ-Al2O3 in a mass ratio of 200:3.2:10 to obtain a mixed solution;
[0033] S2, the obtained mixed solution was kept in a constant temperature water bath at 55°C and magnetically stirred for 12 hours until it was semi-dry;
[0034] S3, then put it into an oven and treat it at a temperature of 105°C for 10 hours;
[0035] S4, after drying, calcining at 500°C in a muffle furnace for 4 hours;
[0036] S5. Grind and sieve to obtain a solid sample with a particle size of 20-40 mesh.
[0037] Example 2
[0038] S1. Mix water, Mg(NO3)2·6H2O and γ-Al2O3 in a mass ratio of 200:6.4:10 to obtain a mixed solution;
[0039] S2, the obtained mixed solution was kept in a constant temperature water bath at 60°C and magnetically stirred for 10 hours until it was semi-dry;
[0040] S3, then put it into an oven and treat it at a temperature of 105°C for 15h;
[0041] S4, after drying, calcining in a muffle furnace at 500°C for 5 hours;
[0042] S5. Grind and sieve to obtain a solid sample with a particle size of 20-40 mesh.
[0043] Example 3
[0044] S1. Mix water, Mg(NO3)2·6H2O and γ-Al2O3 in a mass ratio of 200:12.8:10 to obtain a mixed solution;
[0045] S2, the obtained mixed solution was kept in a constant temperature water bath at 65°C and magnetically stirred for 6 hours until it was semi-dry;
[0046] S3, then put it into an oven and treat it at a temperature of 105°C for 20 hours;
[0047] S4, after drying, calcining in a muffle furnace at 510°C for 3 hours;
[0048] S5. Grind and sieve to obtain a solid sample with a particle size of 20-40 mesh.
[0049] Example 4
[0050] S1. Mix water, Mg(NO3)2·6H2O and γ-Al2O3 in a mass ratio of 200:19.2:10 to obtain a mixed solution;
[0051] S2, the obtained mixed solution was kept in a constant temperature water bath at 60°C and magnetically stirred for 10 hours until it was semi-dry;
[0052] S3, then put it into an oven and treat it at a temperature of 105°C for 15h;
[0053] S4, after drying, calcined in a muffle furnace at 505°C for 4 hours;
[0054] S5. Grind and sieve to obtain a solid sample with a particle size of 20-40 mesh.
[0055] Comparative Example 1
[0056] The pure magnesium oxide powder is granulated, ground and sieved to obtain particles larger than 20 mesh.
[0057] Comparative Example 2
[0058] Except for using Ca(OH)2 raw material to replace the Mg(NO3)2·6H2O raw material in Example 2, the rest is basically the same as Example 1.
[0059] Comparative Example 3
[0060] The γ-Al2O3 raw material of Example 2 is replaced by α-Al2O3, and the rest is basically the same as Example 1.
[0061] The present invention uses nitrogen adsorption-desorption isotherms to measure the BET specific surface area, pore volume and pore diameter of the dechlorination agents prepared in Examples 1-4 and Comparative Examples 1-3. The results are shown in Table 1.
[0062] Table 1 Physical and chemical properties of the dechlorinating agents obtained in Examples 1-4 and Comparative Examples 1-3
[0063] Types of dechlorinating agents <![CDATA[BET specific surface area / (m 2 / g)]]> <![CDATA[Pore volume / (cm 3 / g)]]> Pore diameter / nm Example 1 204.20 0.49 10.23 Example 2 210.53 0.53 10.01 Example 3 193.59 0.47 10.27 Example 4 184.62 0.33 10.36 Comparative Example 1 10.7 0.07 20.10 Comparative Example 2 23.14 0.14 18.14 Comparative Example 3 90.7 0.29 13.24
[0064] It can be seen from Table 1 that the magnesium oxide type dechlorination agent loaded with γ-Al2O3 has a higher specific surface area and pore volume. The BET specific surface area of the γ-Al2O3 loaded magnesium oxide dechlorination agent prepared by the present invention is 180-215m 2 / g, pore volume is 0.30-0.55cm 3 / g, the pore size is 10-10.5nm, which significantly increases the specific surface area of MgO and has a developed pore structure.
[0065] At the same time, the present invention also tests the dechlorination effects of the dechlorinating agents obtained in Examples 1-4 and Comparative Examples 1-3. The test results are shown in Table 2.
[0066] The test method is as follows: the dechlorinating agent of each embodiment and the reference example is placed on a fixed bed test bench for dechlorination characteristic detection. At a fixed bed temperature of 150°C, the total gas volume is uniformly controlled to be 1000mL / min, the HCl concentration is 150ppm, the inner diameter of the quartz reactor is 8mm, the dechlorinating agent dosage is 0.1g, the carrier gas is high-purity nitrogen, and the dechlorination treatment time is 5min. The dechlorination effect is evaluated by removal rate, removal rate = (1-penetration rate) × 100%, wherein the penetration rate is defined as the ratio of the amount of chloride ions enriched at the outlet of the reactor to the total amount of chloride ions in HCl during the test time.
[0067] Table 2 Dechlorination effect of the dechlorinating agents obtained in Examples 1-4 and Comparative Examples 1-3
[0068] Types of dechlorinating agents HCl removal rate within 5 minutes Example 1 51.7% Example 2 71.6% Example 3 61.4% Example 4 54.4% Comparative Example 1 31.2% Comparative Example 2 35.8% Comparative Example 3 41.7%
[0069] As shown in Table 2, after being loaded with γ-Al2O3, MgO has a higher HCl removal efficiency, but the removal efficiency is different at different loading rates. The main reason may be that the γ-Al2O3 skeleton plays an important role in carrying active components in the dechlorinator, providing a porous and loose environment for MgO, thereby increasing the mass transfer rate of the gas inside the dechlorinator and exposing more active sites. Therefore, with the increase of Mg content, the dechlorination effect of the dechlorinator increases first and then decreases. This may be because, when the Mg content is increased to a certain level, on the one hand, the pores between the Al2O3 skeletons will be blocked by active components, and the gas diffusion in the dechlorinator encounters greater resistance. On the other hand, the active sites of the dechlorinator are blocked with each other and cannot contact HCl, which reduces the number of active sites and thus reduces the dechlorination efficiency.
[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An application of a supported magnesium oxide dechlorinating agent, characterized in that: The supported magnesium oxide dechlorinating agent dechlorinates the flue gas at a temperature of 150-200°C; The preparation method of the supported magnesium oxide dechlorinating agent comprises the following steps: Mixing water, magnesium salt and γ-Al2O3 to obtain a mixed solution, stirring, drying, calcining and grinding the obtained mixed solution in sequence to obtain the supported magnesium oxide dechlorination agent; Wherein, the mass ratio of water, magnesium salt and γ-Al2O3 is 200: (3.2-19.2): 10; During the drying, the temperature is controlled at 100-110°C and the time is 10-20 h; During the calcination, the temperature is controlled at 500-510° C. and the time is 3-5 h in a nitrogen atmosphere; After grinding, pass through a 20-40 mesh sieve; The BET specific surface area of the supported magnesium oxide dechlorinating agent is 180-215 m 2 / g, pore volume is 0.30-0.55cm 3 / g, pore size is 10-10.5nm.
2. The use of a supported magnesium oxide dechlorinating agent according to claim 1, characterized in that: The magnesium salt is Mg(NO3)2·6H2O or Mg(CH3COO)2·4H2O.
3. The use of the supported magnesium oxide dechlorinating agent according to claim 1, characterized in that: During the stirring, magnetic stirring is performed in a water bath at 55-65° C. for 2-12 h.