Method for producing printed matter and printed matter
By using a patterned pressing roller and active energy ray curing ink during the printing process, the contradiction between printing concentration and grayscale expression is solved, the glossiness and wear resistance of the printed material are improved, and the high quality is achieved Quality printing effect.
Patent Information
- Application Number
- CN202180021924.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-23
- Filing Date
- 2021-03-25
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-03-25
AI Technical Summary
When the existing active energy ray curing lithographic printing ink increases the printing concentration, it is easy to cause the grayscale performance to deteriorate and the leveling property to be poor, affecting the quality of the printed product.
A printing method with a patterned pressing cylinder in contact with the transfer surface is adopted, by selectively smoothing the solid portion, combining the instantaneous curing characteristics of the active energy ray curing ink, the printing concentration is improved while maintaining grayscale expression.
It is achieved to improve the printing concentration without damaging grayscale expression, enhance the gloss and wear resistance of the printed material, and to take into account both gloss and obscurity, significantly improve the smoothness and durability of the printed material.
Smart Images

Figure CN115362064B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing a printed matter. Background Art
[0002] As the world's population increases, the demand for flexible packaging used in the packaging of food and daily necessities is expected to expand in the future. Flexible packaging refers to printing on a plastic film, which is laminated after printing and processed into a bag shape. At present, in gravure printing, which has become the mainstream in flexible packaging printing, a printed material with a distinct appearance can be obtained, but since a large amount of ink containing solvent is used, a large amount of energy is required in the drying or exhaust treatment of the ink solvent, and the environmental load is also large. In addition, from the previous mass production and large consumption to small batches, multiple varieties, and short delivery periods, the market demand has changed, and the price of plate fees and plate making fees is high, which also leads to an increase in the production cost of gravure printing that is good at large batches. Therefore, in recent years, attempts have been made to implement flexible packaging printing using lithography, which is cheap in price and has an advantage in cost from the perspective of small batches and short delivery periods (patent document 1).
[0003] Lithography is a widely popular printing method as a system for supplying printed matter at high speed, in large quantities and at low cost. In addition, in recent years, from the viewpoint of coping with environmental problems, there is a demand for reducing the volatile components contained in lithographic ink. Therefore, the use of lithographic ink (hereinafter referred to as active energy ray-curable lithographic ink) that does not contain volatile components and is instantly cured by irradiation with active energy rays is being promoted (patent document 2). In flexible packaging printing, since printing is performed by roller to roller, the quick-drying property of ink is important. In addition to the advantages in the environment, active energy ray-curable lithography using active energy ray-curable lithographic ink also shortens the drying process without using thermal energy, thus saving energy and having high productivity.
[0004] Generally, the viscosity of active energy ray-curable lithographic ink is high, and the leveling property is poor due to instant curing, and the printing concentration is easily lower than that of conventional gravure printing. When the ink supply is increased for high printing concentration, the adhesion of the film blank is reduced due to the deterioration of printing adaptability such as dirt and the thickening of the film. Therefore, attempts have been made to reduce the unevenness of the ink layer surface by configuring a full-surface roller during the period from printing to curing (Patent Document 3).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2004-358788
[0008] Patent Document 2: Japanese Patent Application Publication No. 2017-132895
[0009] Patent Document 3: Japanese Patent Application Publication No. 2009-274432 Summary of the invention
[0010] According to the technology disclosed in Patent Document 3, although the printing density of the solid part is improved, the halftone dot part is larger than the setting (hereinafter referred to as dot gain), and the grayscale expression is deteriorated due to tone jumps in shadows and highlights.
[0011] Therefore, an object of the present invention is to provide a method for producing a printed article, which uses an active energy ray-curable ink and can increase the printing density without impairing grayscale expression properties.
[0012] The present inventors have disclosed the following invention of a production method in order to solve the above-mentioned problems.
[0013] (1) A method for producing a printed article, comprising: a transfer step of transferring ink to a transfer surface of a printed article; and a pressing step of bringing a pressing roller into contact with the transfer surface to which the ink has been transferred, wherein at least one of the pressing rollers has a patterned pressing portion.
[0014] Furthermore, as a preferred embodiment of the present invention, there is the following production method.
[0015] (2) According to the method for producing a printed matter described in (1) above, 80% or more of the area of the top surface of the patterned pressing portion corresponds to a solid portion transferred to the transfer surface before the pressing step.
[0016] (3) According to the method for producing a printed matter described in (1) or (2) above, the pressing force of the pressing roller having the patterned pressing portion and the impression roller facing the pressing roller having the patterned pressing portion and sandwiching the printed matter is 100 N / cm 2 Above and 700N / cm 2 the following.
[0017] (4) The method for producing a printed article according to any one of (1) to (3) above, wherein the surface roughness Ra of the top surface of the patterned pressing portion is 0.30 μm or less.
[0018] (5) The method for producing a printed article according to any one of (1) to (4) above, wherein the surface roughness Rz of the top surface of the patterned pressing portion is 2.00 μm or less.
[0019] (6) The method for producing a printed article according to any one of (1) to (5) above, wherein the surface free energy of the top surface of the patterned pressing portion is 36 mN / m or more and 50 mN / m or less.
[0020] (7) According to the method for producing a printed matter according to any one of (1) to (6) above, the pressing roller having the patterned pressing portion is a roller on which at least one selected from an offset printing plate, a flexographic printing plate, a resin relief plate and a rubber blanket is installed.
[0021] (8) The method for producing a printed matter according to (7) above, wherein the offset printing plate is a waterless plate.
[0022] (9) In the method for producing a printed matter according to (7) or (8) above, the pressing portion is an ink smoothing material attached to the blanket.
[0023] (10) The method for producing a printed matter according to any one of the above, further comprising an irradiation step of irradiating the ink with the active energy ray after the transfer step and the pressing step.
[0024] (11) The method for producing a printed material according to any one of (1) to (10) above, wherein the printed material is a non-absorbent blank.
[0025] (12) According to the method for producing a printed matter described in (11) above, the non-absorbing blank is a film.
[0026] (13) The method for producing a printed matter according to (12) above, wherein the film has a thickness of 5 μm or more and 50 μm or less.
[0027] (14) According to the method for manufacturing a printed matter described in any one of (1) to (10) above, in the transfer step and the pressing step, a single impression roller is used to sandwich the printed matter facing the roller for transferring ink and the pressing roller.
[0028] (15) According to any one of the above (1) to (14), the loss tangent (tan δ) of the ink in the pressing step at 25° C. and a measurement frequency of 10 rad / s is greater than or equal to 1.0 and less than or equal to 4.0.
[0029] (16) According to any one of the above-mentioned (1) to (15), the transfer step is performed multiple times, and the ink used in at least the first transfer step among the multiple times is at least one of white ink and thickening ink.
[0030] (17) The method for manufacturing a printed matter according to any one of (1) to (16) above includes another transfer step after a pressing step using a pressing roller having the patterned pressing portion, and another pressing step using another pressing roller having a patterned pressing portion after the transfer step.
[0031] (18) The method for producing a printed matter according to any one of (1) to (17) above further includes another transfer step between the pressing step performed using a pressing roller having the patterned pressing portion and the irradiation step.
[0032] In addition, the present inventors disclose the invention of the following printed matter.
[0033] (19) A printed matter, wherein a surface roughness Ra of a solid portion on the printed matter is 0.10 μm or more and 0.50 μm or less, and a Young's modulus of an arbitrary ink film on the printed matter is 3 GPa or more and 5 GPa or less.
[0034] According to the method for producing a printed matter of the present invention, by selectively smoothing only the solid part of the printed matter, the printing density can be increased without impairing the grayscale expression. Moreover, by selective smoothing, a wide range of printing expressions in which glossiness and matteness coexist can be easily given. In addition, the obtained printed matter exhibits excellent glossiness and abrasion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a diagram showing images of printing plates used in printing methods 1, 2, and 3 in Examples.
[0036] Figure 2 This is a diagram showing images of printing plates used in printing methods 4, 5, and 6 in Examples.
[0037] Figure 3 It means Figure 2 A diagram showing how smoothed materials are selectively pasted corresponding to the image. DETAILED DESCRIPTION
[0038] The present invention is described in detail below. Furthermore, in the present invention, "above" means the same as or greater than the numerical value shown here. In addition, "below" means the same as or less than the numerical value shown here. In addition, "(meth)acrylate" refers to a general term including acrylate and methacrylate.
[0039] The present invention is a method for manufacturing printed matter, which comprises in sequence: a transfer process of transferring ink to a transferred surface of a printed matter, and a pressing process of bringing a pressing roller into contact with the transferred surface to which the ink is transferred, wherein at least one of the pressing rollers has a patterned pressing portion.
[0040] (Printed material)
[0041] In the method for producing printed matter of the present invention, as the printed matter, coated paper such as art paper, coated paper, cast-coated paper, uncoated paper such as premium paper, newspaper paper, Japanese paper, synthetic paper, aluminum-deposited paper, metal, film, and other non-absorbent blanks can be used. Among them, non-absorbent blanks with low ink transfer properties and which do not penetrate ink after transfer are preferred, and films with low ink transfer properties are particularly preferred.
[0042] Examples of the film include polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyesters such as polylactic acid, polyamides, polyimides, polyalkyl (meth) acrylates, polystyrene, poly-α-methylstyrene, polycarbonates, polyvinyl alcohol, polyvinyl acetal, polyvinyl chloride, polyvinylidene fluoride, etc. These plastic films may be subjected to surface treatments such as calcination, easy-adhesion coating, and chemical vapor deposition.
[0043] From the viewpoint of the mechanical strength of the film required for printing, the thickness of the film is preferably 5 μm or more, more preferably 10 μm or more, and preferably 50 μm or less, more preferably 30 μm or less, as the film cost is low.
[0044] As the form of the non-printed material used in the method for producing a printed material of the present invention, either a single sheet or a roll can be used. When printing is performed on a thin film for a flexible package, it is preferred to use a roll film and perform roll-to-roll printing.
[0045] (ink)
[0046] In the method for producing printed matter of the present invention, the ink may be any known ink of oxidative polymerization type, drying type, active energy ray curing type, such as flexible ink, offset ink, gravure ink, screen ink, ink jet ink, etc. In particular, due to the characteristics of instant curing, active energy ray curing type ink with poor leveling property and offset ink with high viscosity are preferred because they can obtain a high smoothing effect in the pressing process described later. In addition, ink for waterless plate printing among offset inks may also be used. In addition, commercial products may be used, and synthetic products may also be used.
[0047] Specific examples of commercially available active energy ray-curable inks include electron beam-curable inks such as EC DEVELOPMENT manufactured by Sun Chemical and XCURA EVO manufactured by Flint.
[0048] The synthetic active energy ray-curable ink is obtained by adding a pigment and an auxiliary agent to a resin varnish obtained by dissolving a resin in a multifunctional (meth)acrylate, and kneading the mixture using a three-roll mill.
[0049] Examples of the resin include acrylic resins, polyurethane resins, phthalate resins, etc. Commercial products or synthetic products can be used. Specific examples of commercial products include the "Hirose Ichi" (registered trademark) series manufactured by Seiko PMC Co., Ltd. for acrylic resins, and the "Daiso Dap" (registered trademark) series and "Daiso Isodap" (registered trademark) manufactured by Osaka Soda Co., Ltd. for phthalate resins.
[0050] In the case of synthetic resins, if it is an acrylic resin, it can be obtained by polymerizing (meth)acrylate monomers alone or by mixing two or more kinds in an organic solvent in the presence of a polymerization initiator. In addition, styrene, α-methylstyrene, etc. can also be copolymerized.
[0051] As the (meth)acrylate monomer, linear or branched alkyl (meth)acrylates having 1 to 24 carbon atoms can be used. As alicyclic alkyl (meth)acrylates, isobornyl (meth)acrylate, norbornyl (meth)acrylate, norbornane-2-methanol (meth)acrylate, cyclohexyl (meth)acrylate, tricyclopentyl (meth)acrylate, tricyclopentyloxy (meth)acrylate, tricyclodecane monohydroxymethyl (meth)acrylate can be used. As carboxyl group-containing (meth)acrylates, (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, vinyl acetate, etc. can be used. As hydroxyl group-containing (meth)acrylates, 2-hydroxyethyl acrylate, 2-hydroxybutyl acrylate, etc. can be used. As amino group-containing (meth)acrylates, dimethylaminoethyl methacrylate, dimethylaminobutyl methacrylate, etc. can be used. As sulfonic group-containing (meth)acrylates, acrylamidotert-butylsulfonic acid ester can be used. As phosphoric acid group-containing (meth)acrylates, 2-methacryloyloxyethyl acid phosphate can be used.
[0052] If it is a polyurethane resin, it can be obtained by mixing one or more polyols and polyisocyanates respectively and carrying out a polycondensation reaction in an organic solvent in the presence of a condensing agent. Examples of polyols include polyester polyols, polycarbonate polyols, polyether polyols, etc. Examples of polyisocyanates include polyurethane polyisocyanates, isocyanurates, etc.
[0053] If it is a phthalate resin, it can be obtained by using diallyl orthophthalate or diallyl isophthalate alone or by mixing two kinds and carrying out a polymerization reaction in an organic solvent in the presence of a polymerization initiator.
[0054] Examples of the polyfunctional (meth)acrylate include diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, glycerol di(meth)acrylate, pentaerythritol di(meth)acrylate, diglycerol di(meth)acrylate, di(trimethylolpropane) di(meth)acrylate, dicyclopentadiene tricyclodecane dimethanol di(meth)acrylate, and ethylene oxide adducts, propylene oxide adducts, and tetraethylene oxide adducts thereof. Examples of the polyfunctional (meth)acrylate include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and di(trimethylolpropane) di(meth)acrylate. Examples of the present invention include tri(meth)acrylate, glycerol tri(meth)acrylate, isocyanurate tri(meth)acrylate, ethylene oxide adducts and propylene oxide adducts thereof; examples of tetrafunctional compounds include di(trimethylolpropane) tetra(meth)acrylate, diglycerol tetra(meth)acrylate, ethylene oxide adducts and propylene oxide adducts thereof; and examples of pentafunctional compounds or higher include dipentaerythritol hexa(meth)acrylate, ethylene oxide adducts and propylene oxide adducts thereof.
[0055] Examples of the pigment include phthalocyanine pigments, soluble azo pigments, insoluble azo pigments, lake pigments, quinacridone pigments, isoindoline pigments, threne pigments, metal complex pigments, titanium oxide, zinc oxide, alumina white, calcium carbonate, barium sulfate, red iron, cadmium red, chrome yellow, zinc yellow, Prussian blue, ultramarine, oxide-coated glass powder, oxide-coated mica, oxide-coated metal particles, aluminum powder, gold powder, silver powder, copper powder, zinc powder, stainless steel powder, nickel powder, organic bentonite, iron oxide, carbon black, graphite, and the like.
[0056] In addition, as the pigment, mica (hydrous potassium aluminum silicate), talc (magnesium silicate) and the like which are colorless extender pigments may be used, and a thickening ink containing no pigment may be used.
[0057] Furthermore, additives such as a photopolymerization initiator, wax, a pigment dispersant, a defoaming agent, and a leveling agent may be used for the ink.
[0058] Although an ultraviolet curing ink containing a photopolymerization initiator may be used, since decomposed products and unreacted products of the photopolymerization initiator may cause odor and contamination of the contents, a radiation curing ink containing no such products is more preferable.
[0059] In addition, the ink used in the present invention preferably has a loss tangent (tanδ) value of 1.0 or more and 4.0 or less at 25°C and a measuring frequency of 10 rad / s. The value of the loss tangent (tanδ, hereinafter referred to as "tanδ") is measured by a sine wave vibration method using a dynamic viscoelasticity measuring device. tanδ is the ratio G" / G' of the storage elastic modulus (G') to the loss elastic modulus (G"). The smaller the value of tanδ, the stronger the property of the ink to recover to its original state relative to deformation. On the other hand, the larger the value of tanδ, the stronger the property of the ink to follow deformation. Generally, a value less than 1 means that it is solid and has low fluidity, and the larger the value, the higher the fluidity. Under low shear at a measuring frequency of 10 rad / s, by making tanδ greater than 1.0, more preferably greater than 2.0, the ink can be deformed by pressing. In addition, by making it less than 4.0, more preferably less than 3.0, the ink can be prevented from leveling in the non-drawing line part, and a smoothing effect based on pressing can be effectively obtained.
[0060] (Transfer process)
[0061] In the transfer process, the ink is transferred to the transfer surface of the printed object.
[0062] Generally, a color print requires a printing unit for transferring ink in the same number of colors to be printed. In the printing unit for each color, the ink for the image line is transferred from an ink roller to a transfer surface of the printed material via a rubber blanket depending on the printing plate and the printing method.
[0063] In the transfer process, as a method of transferring ink to the printed surface, it can be transferred to the printed surface by a known method such as flexographic printing, offset printing, gravure printing, screen printing, inkjet printing, varnish coater, rod coater, etc. In particular, in the offset printing method, the viscosity of the ink is usually high and the leveling property is low, so the method for manufacturing the printed matter of the present invention can be applied with a significant effect. In the offset printing method, waterless offset printing is also preferred, which does not have the concern that the smoothing effect is reduced due to the adhesion of wet water to the pressing roller having the patterned pressing portion.
[0064] (Pressing process)
[0065] In the pressing step, the pressing roller is brought into contact with the transfer surface to which the ink has been transferred.
[0066] Generally, since the image pattern is different for each color to be printed, the uncured ink on the transferred surface transferred by the first printing unit will contact the rubber blanket surface corresponding to the non-lined part of the image in the later printing unit. Therefore, the rubber blanket roller acts as a pressing roller, and although it has the effect of smoothing the surface of the uncured ink, the effect is small because the rubber blanket surface generally has unevenness. In addition, depending on the number of printing units of the printing press, sometimes there are empty printing units that are not used. For ink smoothing, the rubber blanket in the empty printing unit can also be used as a pressing roller. However, its effect is still limited by the unevenness of the rubber blanket surface. The full-surface roller disclosed in Patent Document 3 has a high effect of further reducing the unevenness of the printed surface by a roller with a rigid and smooth surface. However, in any of these methods, in order to smooth the entire surface of the printed matter, not only the dot gain of the solid part where the printing density is to be increased becomes larger, but also the dot gain of the halftone part becomes larger, and the grayscale expression such as tone jump caused by shadows and highlights is deteriorated. In addition, the higher the smoothing effect of reducing unevenness, the greater the dot gain of the blanket or roller, because the dots are pressed and aligned by the same principle as the solid part.
[0067] (Pressure roller with patterned pressure portion)
[0068] In the method for manufacturing printed matter of the present invention, it is important that at least one of the pressing rollers has a patterned pressing portion. By having a patterned pressing portion in the area in contact with the transferred surface, it is possible to selectively set the portion to be smoothed and the portion not to be smoothed in the transferred surface. The smoothing effect is further improved when the pressing portion, which has a smaller concave-convex shape than the rubber blanket surface, contacts the uncured ink. In addition, the patterned pressing portion is different from the setting of the roller and the replacement of the rubber blanket disclosed in Patent Document 3. The presence or absence of contact with the transferred surface is selected by patterning, thereby being divided into a solid portion to be smoothed and a dot portion that is not smoothed and maintains grayscale expression. Moreover, the method for manufacturing printed matter of the present invention can also utilize the existing rubber blanket cylinder of the printing press, without the need for equipment modification, and only the patterned pressing portion of the existing rubber blanket cylinder or the rubber blanket surface needs to be disassembled, so the simplicity is also excellent.
[0069] In the method for manufacturing a printed matter of the present invention, preferably, more than 80% of the area of the pressing portion in contact with the transfer surface corresponds to the solid portion transferred to the transfer surface before the pressing step. By making more than 80%, more preferably more than 90%, and even more preferably 100% of the area of the pressing portion correspond to the solid portion, both the smoothing effect and the grayscale expression can be effectively achieved.
[0070] In order to improve the smoothing effect, the surface roughness of the top surface of the pressing portion is preferably smaller than that of the rubber blanket surface. The surface roughness Ra based on the arithmetic mean of the top surface of the pressing portion is preferably 0.30 μm or less from the perspective of a high effect of smoothing the unevenness of the ink surface when in contact with the uncured ink surface. In addition, the surface roughness Rz based on the ten-point average is preferably 2.00 μm or less from the perspective of reducing the blanks generated on the ink surface due to local unevenness. These surface roughness parameters are specified in accordance with JIS B0601:2013.
[0071] The surface free energy of the top surface of the pressing portion is preferably 36mN / m or more and 50mN / m or less. By setting it to 36mN / m or more, more preferably 38mN / m or more, and further preferably 40mN / m or more, the pressing portion receives an excess amount of uncured ink that tends to be excessively supplied to the transferred surface after just starting printing. Therefore, for the subsequent transferred surface, the excess amount of ink first received by the pressing portion can be supplied to the transferred surface, and the printing concentration is improved. On the other hand, by setting it to 50mN / m or less, more preferably 48mN / m or less, and further preferably 46mN / m or less, the ink transferability to the printed object is improved compared to the pressing roller with a patterned pressing portion.
[0072] In the method for manufacturing printed matter of the present invention, as a pressing roller having a patterned pressing portion, it is preferred that a roller is installed with at least one selected from an offset printing plate, a flexographic printing plate, a resin relief plate and a rubber blanket. By exposing and developing the offset printing plate, the flexographic printing plate, the resin relief plate (hereinafter, they are also referred to as "the original plate of the pressing portion") in correspondence with the solid portion of the color of the printed image to be smoothed, the solid portion can be selectively patterned. At this time, in order to make the convex portion of the original plate of the pressing portion consistent with the solid portion of the color of the printed image to be smoothed, when an offset printing plate as a flat relief plate and a flexographic printing plate or a resin relief plate as a relief plate are used as the original plate of the pressing portion, the line portion corresponds to the solid portion of the printed image. On the other hand, when a waterless planographic printing plate as a flat concave plate is used as the original plate of the pressing portion, the non-line portion corresponds to the solid portion of the printed image. The original plates of these pressing portions can be directly mounted on the roller, or an adhesive layer can be provided on the back of the original plate and mounted on the rubber blanket mounted on the rubber blanket roller.
[0073] Among them, as the original plate of the pressing portion, it is preferable to use a waterless plate whose outermost surface is made of silicone rubber, which easily satisfies the above-mentioned surface roughness Ra, has high smoothness, and easily rebounds ink.
[0074] In addition, when using a rubber blanket, it is preferable to paste and use an ink smoothing material. The ink smoothing material refers to a smoothing member that has the effect of smoothing the ink by pressing the ink. Specifically, it is preferable to have the aforementioned surface roughness Ra. In addition, it is preferable to have the aforementioned surface free energy. Since the rubber blanket alone has unevenness on the surface, the smoothing effect is small, but by pasting the ink smoothing material, the smoothing effect in the pressing process can be improved. In addition, it is also an advantage that the smoothing effect can be controlled according to the chemical and physical properties of the pasted ink smoothing material.
[0075] As a method for selectively pasting the ink smoothing material corresponding to the solid part of the printed material, in the case of an image with a mixture of solid and halftone dots, an adhesive layer is provided on the back of the ink smoothing material only in accordance with the solid part of the color of the printed image to be smoothed and installed on the surface of the rubber blanket.
[0076] In addition, the ink smoothing material may be pasted on the original plate of the patterned pressing portion for use. In particular, if the image is a background color with almost no dots, as a simpler method, the ink smoothing material may be cut into a rough shape covering the solid part of the color to be smoothed of the printed image and attached to the blanket cylinder or the blanket surface.
[0077] The ink smoothing material preferably has an adhesive layer on its back side (the side opposite to the side in contact with the printed matter). The adhesive layer allows easy attachment to the blanket cylinder or blanket surface of an existing printing press.
[0078] The adhesive strength of the adhesive layer of the ink smoothing material is preferably 1N / 50mm or more, which allows the ink smoothing material to be attached to the blanket surface and not peel off during printing. In addition, when peeling from the blanket surface after use, it is preferably 15N / 50mm or less, which does not apply a work load. In addition, when peeling from the blanket surface, the adhesive layer is not likely to remain, but cleaning becomes simple, which is preferred.
[0079] In the method for producing printed matter of the present invention, from the viewpoint of ink transferability and durability, the rubber blanket preferably has at least one ink transfer layer, base fabric layer, and compression layer, respectively. In order to combine adjacent layers, an adhesive layer may be provided between the layers.
[0080] The material of the ink transfer layer is not particularly limited, and resins such as polyimide resin, polyamideimide resin, polyamide resin, polyethylene terephthalate resin, polyethylene naphthalate resin, polycarbonate resin, acrylonitrile-butadiene-styrene (ABS) resin, poly(methyl)acrylate resin, polyvinylidene fluoride resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyvinyl alcohol resin, polyethylene resin, polypropylene resin, polyurethane resin, and rubbers such as ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), acrylonitrile butadiene rubber (NBR), carboxylated acrylonitrile butadiene rubber (XNBR), acrylic rubber (ACM), chloroprene rubber (CR), epoxidized natural rubber (ENR), hydrogenated acrylonitrile butadiene rubber (HNBR), and polyurethane rubber can be appropriately used.
[0081] In addition, in order to attach the rubber blanket to the rubber blanket cylinder, an adhesive layer may be provided on the surface opposite to the ink transfer layer. The material of the adhesive layer is not particularly limited, and thermoplastic resins, thermosetting resins, synthetic rubbers, and natural rubbers may be used appropriately. From the perspective of being able to improve the adhesion between the adjacent layers and the rubber blanket cylinder, polyurethane, acrylic resin, polysulfide, polyvinyl chloride, modified polyolefin, polyurea, butadiene rubber, styrene-butadiene rubber, chloroprene rubber, and silicone rubber are preferably used.
[0082] The compressive stress when the amount of pressure applied to the blanket cylinder is 0.30 mm is preferably 200 N / cm 2 Above and 600N / cm 2 Below. By setting it to 200N / cm 2 More preferably, 250 N / cm 2 More preferably, 300 N / cm 2 The above mentioned properties improve the ink transferability from the blanket cylinder to the film. 2 Below, more preferably 550N / cm 2 Below, more preferably 500N / cm 2 As a result, the load on the printing press can be reduced.
[0083] From the viewpoint of the compressibility of the blanket, the amount of indentation between the blanket cylinder and the film is preferably 0.20 mm to 0.40 mm, more preferably 0.25 mm to 0.38 mm, and even more preferably 0.30 mm to 0.36 mm.
[0084] The thickness of the pressing portion depends on the cylinder manufacturing method of the printing press, but in order to be able to adjust the printing pressure within a commonly used range after installation, the thickness of the pressing portion after installation is preferably 1 mm to 3 mm, which is the same as that of the existing rubber blanket.
[0085] In the method for manufacturing printed matter of the present invention, it is preferred that the impression roller that sandwiches the printed matter facing the roller for transferring ink and the pressing roller is single. By using a single impression roller, even if the printed matter is a thin film, multi-color printing can be performed with high estimation accuracy, and the deviation between the solid part of the printed surface and the patterned pressing part becomes smaller. As a specific mechanism, it is preferred to use a rotary printing press equipped with a central pressure roller. As a specific example of the rotary printing press, among flexible printing presses, "MIRAFLEX" manufactured by Windmoeller & Hoelscher can be cited, and among offset printing presses, CI-8 manufactured by COMEXI can be cited.
[0086] The pressure between the pressing roller and the impression roller that applies pressure to the printed material together with the pressing roller in the pressing step is preferably 100 N / cm, which has a high effect of smoothing the unevenness of the ink surface. 2 More than 200 N / cm 2 More preferably, 300 N / cm 2 In addition, it is preferred that the pressure is not excessively high, i.e. 700 N / cm2, which does not impose an excessive load on the printing press represented by the impression roller or the pressure roller. 2 Below, more preferably 600N / cm 2 , more preferably 500N / cm 2 the following.
[0087] In the method for manufacturing printed matter of the present invention, the transfer step may be performed multiple times, at least one of the multiple times includes a step of transferring the ink into the solid part, and the pressing step is included after the transfer step. By pressing with the pressing part corresponding to the solid part, a smoothing effect can be efficiently obtained.
[0088] It is particularly preferred that at least the first transfer step in the multiple transfer steps is a step of transferring the ink within the solid part, and the pressing step is included after the transfer step. In the manufacture of printed matter, functional inks such as color inks widely including solid parts and thickening inks are initially transferred and applied to the pressing step at an appropriate time, thereby avoiding the dot parts of the ink including a large number of dot parts from being crushed and achieving the smoothing effect of the solid part efficiently.
[0089] In the method for manufacturing printed matter of the present invention, it is preferred that the ink including the solid part to be transferred is at least one of white ink and thickening ink. Although there is no restriction on which color of ink to use, both white ink and thickening ink have very few dots and the solid part is the majority. The white ink is usually a background color with high concealment. By transferring the white ink including the solid part in the interior in at least the initial transfer process among multiple transfer processes, it can be used as a front printing, so it is preferred. In addition, the thickening ink is equivalent to an intermediate layer that is in close contact with both the film as the printed object and other inks, so it is preferably used in at least the initial transfer process among multiple transfer processes.
[0090] The method for manufacturing printed matter of the present invention may also include other transfer processes between the pressing process and the irradiation process. This method is effective when the solid part and the dot part overlap in the printed image. That is, after reducing the unevenness of the solid part of the first ink-brushed solid part by using a pressing roller with a patterned pressing part, the dot part of the later ink-brushed overlaps with the solid part of the first ink-brushed solid part, so that even in the same part, the smoothness of the solid part and the grayscale expression of the dot part can be taken into account. This is different from the process disclosed in Patent Document 3, which uses a full-surface roller to smooth the entire surface of the printed matter only after printing all the colors. It is possible to select a unit of a pressing roller with a patterned pressing part, so that any part of any color can be selectively smoothed. In addition, when the smoothness of the color brushed first is improved, the transferability of the color brushed later overlapping the same part is also improved, so it is preferred.
[0091] In addition, the method for manufacturing printed matter of the present invention preferably includes another transfer process after the pressing process, and includes another pressing process after the transfer process. By implementing the pressing process multiple times, the smoothing effect can be further improved. In addition, in the other pressing process, it is also possible to achieve smoothing with high accuracy and freedom by pressing under the configuration of a pressing roller having a selectively patterned pressing portion corresponding to the ink pattern of the transfer process not long ago. There is no particular restriction on the number of times the pressing process is implemented, but even when using existing equipment, it can be implemented in practice up to the difference between the number of printing units of the printing press and the number of printed colors of the image.
[0092] (Irradiation process)
[0093] In the irradiation step, the transferred ink is irradiated with active energy rays.
[0094] In the method for manufacturing printed matter of the present invention, as active energy ray sources, ultraviolet rays (especially LED-UV), electron beams, gamma rays, etc. can be listed. Radiation such as electron beams or gamma rays generates high-energy secondary electrons in the irradiated substance, excites the surrounding molecules, and generates reactive species represented by free radicals. When the irradiated substance is active energy ray-curable ink, free radicals are generated in the ink, and the free radical polymerization is promoted to form a cured ink film. In particular, electron beams based on low acceleration voltage have sufficient transmittance relative to the thickness of the ink film below 10μm, are endowed with the energy required for curing, do not require special qualifications when used, are easy to handle, and are therefore preferably used.
[0095] The penetration depth of electron beams is determined by the accelerating voltage, so the accelerating voltage of electron beams is preferably 50 kV or more, more preferably 90 kV or more, and even more preferably 110 kV or more, so that a sufficient amount of beams can penetrate the ink film. In addition, as the penetration depth increases, the amount of beams imparted to the inside of the film also increases, so it is preferably 300 kV or less, more preferably 200 kV or less, and even more preferably 150 kV or less.
[0096] In addition, the higher the electron beam irradiation dose, the greater the amount of free radical species generated in the target substance, but on the other hand, the greater the damage to the film, so the irradiation dose is preferably 10 kGy to 100 kGy, more preferably 20 kGy to 50 kGy.
[0097] (Printed material)
[0098] The printed matter of the present invention is characterized in that the surface roughness Ra of the solid part on the printed matter is greater than or equal to 0.10 μm and less than or equal to 0.50 μm, and the Young's modulus of any ink coating on the printed matter is greater than or equal to 3 GPa and less than or equal to 5 GPa. Usually, printed matters using active energy ray curable ink have poor leveling properties due to instant curing, and the surface roughness Ra of the solid part is greater than or equal to 1 μm, but by utilizing the pressing process to reduce the surface unevenness of the ink, the smoothness is achieved comparable to that of conventional gravure printing. By making the surface roughness Ra of the solid part on the printed matter greater than or equal to 0.10 μm and less than or equal to 0.50 μm, the glossiness required in printed matters, particularly in front printing, becomes excellent.
[0099] In addition, generally speaking, active energy ray-curable ink is irradiated with active energy rays, and multifunctional (meth) acrylate is cross-linked by free radical polymerization to form a mesh structure and solidify, so compared with solvent-dried gravure ink and flexible ink, the ink coating becomes hard, so the mechanical properties such as wear resistance and wiping resistance required in the printed matter printed on the front are also excellent. In particular, since the resin in the ink has multiple ethylenically unsaturated groups, it is easy to perform three-dimensional cross-linking, so it is preferred. By making the Young's modulus in the range of more than 3GPa and less than 5GPa, the mechanical strength such as wear resistance and wiping resistance required for front printing can be met, and it is also possible to follow the bending of a certain degree of printed matter.
[0100] Example
[0101] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples.
[0102] <Ink production>
[0103] [Black Ink 1]
[0104] A mixture of 30 parts by mass of "Diiso Dap" (registered trademark) K manufactured by Osaka Soda as diallyl phthalate resin, 25 parts by mass of M600 manufactured by Miwon and 23 parts by mass of M3130 manufactured by Miwon as multifunctional (meth)acrylate, 18 parts by mass of Mogul E manufactured by Cabot as ink pigment, 2 parts by mass of "Microace" P-8 manufactured by Nippon Tak as extender pigment, 1 part by mass of "Disper" BYK2013 manufactured by BYK as dispersant, and 1 part by mass of KTL-4N manufactured by Kitamura as wax was kneaded using a three-roll mill to prepare active energy ray-curable black ink 1. The tan δ of black ink 1 at 25° C. and a measurement frequency of 10 rad / s was 2.8.
[0105] [Black Ink 2]
[0106] Using a three-roll mill, a mixture of 28 parts by mass of "Daisodaup" (registered trademark) manufactured by Osaka Soda, which is a diallyl phthalate resin, 22 parts by mass of M600 manufactured by Miwon Co., Ltd. and 32 parts by mass of M3130 manufactured by Miwon Co., Ltd., both of which are polyfunctional (meth)acrylates, 16 parts by mass of Mogul E manufactured by Cabot Corp., which is an ink pigment, 1 part by mass of "Disper" BYK2013 manufactured by BYK Co., which is a dispersant, and 1 part by mass of KTL-4N manufactured by Kitamura, which is a wax, was kneaded to produce an active energy ray-curable black ink 2. The tanδ of black ink 2 at 25 °C and a measurement frequency of 10 rad / s is 4.6.
[0107] [White ink 1]
[0108] Using a three-roll mill, a mixture of 16 parts by mass of "Hairosuichi" (registered trademark) VS-1259 manufactured by Starlight PMC, which is an acrylic resin, 18 parts by mass of M4004 manufactured by Miwon Co., Ltd. and 17 parts by mass of M262 manufactured by Miwon Co., Ltd., both of which are polyfunctional (meth)acrylates, 45 parts by mass of CR58-2 manufactured by Ishihara Sangyo Co., Ltd., which is a white pigment, 2 parts by mass of "Micro Ace" P-8 manufactured by Nippon Talc Co., Ltd., which is a extender pigment, 1 part by mass of Disper BYK111 manufactured by BYK Co., which is a dispersant, and 1 part by mass of KTL-4N manufactured by Kitamura, which is a wax, was kneaded to produce an active energy ray-curable white ink 1. The tanδ of white ink 1 at 25 °C and a measurement frequency of 10 rad / s is 3.8.
[0109] <Measurement method of tanδ>
[0110] The tanδ of each ink was measured using a rheometer (MCR301 manufactured by Anton Paar) under the conditions of 25 °C, an ink volume of 0.1 ml, a parallel plate diameter of 25 mm, a strain of 5%, and a measurement frequency of 10 rad / s.
[0111] <Blanket material>
[0112] Blanket material 1: T414W (manufactured by Kinyo Co., Ltd., thickness 1.95 mm, compressive stress of 400 N / cm when indented 0.30 mm 2 , surface roughness Ra 1.02 μm, Rz 8.24 μm)
[0113] Blanket material 2: FIT-UV (manufactured by Fujikura Composite Co., Ltd., thickness 1.95 mm, compressive stress of 270 N / cm when indented 0.30 mm2 , surface roughness Ra1.05μm, Rz6.43μm)
[0114] Blanket material 3: EX6300W (manufactured by Jinyang Co., Ltd.), thickness 1.95mm, compression stress 164N / cm when pressed into 0.30mm 2 , surface roughness Ra0.54μm, Rz3.79μm)
[0115] Blanket material 4: T626 (manufactured by Jinyang Co., Ltd., thickness 1.70 mm, compression stress 629 N / cm when pressed into 0.30 mm 2 , surface roughness Ra 0.96μm, Rz 9.80μm).
[0116] <Compression stress>
[0117] The compressive stress of each rubber blanket material when pressed in is measured by the following method. Prepare a 30mm×30mm square rubber blanket material and stick it on the compression disk of a universal material testing machine (AG-50kNXplus, manufactured by Shimadzu Corporation). As measuring terminals, a compression pressure plate (upper) (size: 50mm diameter) and a compression disk (lower) (size: 200mm diameter) are used. The compression disk (lower) is fixed and measured. A load is applied to the rubber blanket material until the pressing speed reaches 1mm / min and the maximum load reaches 13.5kN (assuming the maximum stress is 15MPa). The moving distance of the compression pressure plate (upper) is measured as the pressing amount. The load value measured when the pressing amount is 0.30mm is converted into the unit of split pressure based on the area of the rubber blanket material. Repeat the above measurement three times and calculate their average value.
[0118] <Members of the pressing section>
[0119] [Member 1 of the pressing portion]
[0120] UTD-10B (manufactured by Nitto Denko, thickness 10 μm, adhesive force 5.8 N / 50 mm) was pasted on the back of "LumiLa" (registered trademark) S10 (manufactured by Toray Co., Ltd., thickness 50 μm, surface roughness Ra 0.06 μm, Rz 0.47 μm, surface free energy 44 mN / m) as an adhesive layer. The ink smoothing material was used as component 1 of the pressing portion.
[0121] [Member 2 of the pressing portion]
[0122] SP-PET-O3-BU (Mitsuei Chemicals Toselo Co., Ltd., thickness 75 μm, surface roughness Ra 0.05 μm, Rz 0.26 μm, surface free energy 30 mN / m, adhesive force 0.6 N / 50 mm) was used as the ink smoothing material.
[0123] [Member 3 of the pressing portion]
[0124] Scratched tab 647 (manufactured by Teraoka Corporation, thickness 80 μm, surface roughness Ra 0.12 μm, Rz 0.40 μm, surface free energy 36 mN / m, adhesive force 15 N / 50 mm) was used as the ink smoothing material. The ink smoothing material was used as the member 3 of the pressing portion.
[0125] [Member 4 of the pressing portion]
[0126] An adhesive layer UTD-10B (manufactured by Nitto Denko, thickness 10 μm, adhesive force 5.8 N / 50 mm) is pasted on the back of "LumiLa" (registered trademark) X42 (manufactured by Toray Co., Ltd., thickness 50 μm, surface roughness Ra 0.32 μm, Rz 2.50 μm, surface free energy 42 mN / m) as an ink smoothing material. The ink smoothing material is used as component 4 of the pressing portion.
[0127] [Member 5 of the pressing portion]
[0128] UTD-30B (manufactured by Nitto Denko, thickness 30 μm, adhesive force 22 N / 50 mm) was pasted on the back of "Eval" (registered trademark) EF-F (manufactured by Kuraray Co., Ltd., thickness 50 μm, surface roughness Ra 0.10 μm, Rz 0.37 μm, surface free energy 54 mN / m) as an adhesive layer as an ink smoothing material. The ink smoothing material was used as component 5 of the pressing portion.
[0129] [Member 6 of the pressing portion]
[0130] A plate was prepared by exposing and developing a waterless planographic original plate (TAC-VT4 manufactured by Toray Co., Ltd., thickness 240 μm) so that the portion to be the pressing portion remained as a convex portion. UTD-10B (manufactured by Nitto Denko, thickness 10 μm, adhesive force 5.8 N / 50 mm) was attached to the back of the obtained plate as an adhesive layer, which served as the member 6 of the pressing portion.
[0131] [Member 7 of the pressing portion]
[0132] A plate was made by exposing and developing a resin relief plate (Toray Co., Ltd., "Toray" K-type) in such a way that the predetermined portion to be the pressing portion remained as a convex portion. UTD-10B (Nitto Denko, thickness 10 μm, adhesive strength 5.8 N / 50 mm) was pasted on the back of the obtained plate as an adhesive layer, which served as component 7 of the pressing portion.
[0133] <Surface roughness>
[0134] The surface roughness of the member of each pressing portion was measured in accordance with JIS B0601-2013. Using a laser microscope (VK-X210 manufactured by Keyence Corporation), 10 random locations were measured at a magnification of 20 and a resolution of 0.1 μm, and the average value was calculated.
[0135] <Surface free energy>
[0136] The surface free energy of each pressing member was measured by a drop method using an automatic contact angle meter (Drop Master DM-500, manufactured by Kyowa Interface Science Co., Ltd.) in each solvent of water, ethylene glycol, and glycerin, and the surface free energy of the ink was calculated from the extended matrix.
[0137] <Adhesion>
[0138] The adhesive strength of each ink smoothing material was measured by peeling a 50 mm wide sample affixed to a stainless steel substrate at 180° at 300 mm / min using a Tensilon universal testing machine (RTG-1210 manufactured by Olientech Co., Ltd.).
[0139] <Preparation of printed version>
[0140] The waterless planographic printing plate (TAC-VT4 manufactured by Toray Co., Ltd.) was used to produce Figure 1 Images 1, 2, Figure 2 Images 3 and 4 in the figure correspond to the waterless planographic printing plates. Figure 1 Image 1 in FIG. 1 has a black (ink) solid portion and a 50% halftone dot portion. Figure 1 Image 2 in the image has only the white solid portion. Figure 2 Image 3 in FIG. 1 has a black solid portion and 50% dots. Figure 2 Image 4 in the image has only the white solid portion.
[0141] <Preparation of the press roller>
[0142] The rubber materials 1 to 4 with different compression characteristics were used as the base, and the pressing part was mounted. A total of 14 types of pressing rollers were prepared, including 13 types of pressing rollers with patterned pressing parts and one type of pressing roller with no patterned pressing part. The patterning of the pressing part was as follows, and the correspondence with the pressing roller is shown in Table 1.
[0143] [Pattern 1]
[0144] Only with Figure 1 The patterning is performed so that the portion corresponding to the solid portion of the ink image 1 in the image contacts the pressing portion. The ratio of the area of the pressing portion corresponding to the solid portion (hereinafter also referred to as "solid area ratio") is 100%.
[0145] [Pattern 2]
[0146] Only with Figure 2 The patterning is performed so that the portion corresponding to the solid portion of the ink image 3 in the image contacts the pressing portion. The solid area ratio of the pressing portion is 100%.
[0147] [Pattern 3]
[0148] Only in Figure 2 The ink image 3 in the image is not the halftone dot part and is Figure 2 The solid part of the white image 4 in the image is patterned in such a way that the part corresponding to the solid part contacts the pressing part ( Figure 3 ). The solid area ratio of the pressing portion is 100%.
[0149] [Pattern 4]
[0150] Only with Figure 2 The patterning is performed so that the portion corresponding to the solid portion of the white image 4 in the image contacts the pressing portion. The solid area ratio of the pressing portion is 100%.
[0151] [Pattern 5]
[0152] The pressing portion is not patterned at a specific position, and the pressing portion contacts the entire surface of the printed object. Figure 1 The ink color image 1 is 78%, compared to Figure 2 The ink color image 3 in is 13%.
[0153]
[0154] In addition, regarding the surface roughness Ra and Rz and the surface free energy in Table 1, the surface roughness and surface free energy of the pressing portion are shown for the pressing roller, and the surface roughness of the blanket material is shown for the pressing roller 14 which is a member without a pressing portion.
[0155] <Printing test>
[0156] The common structure of the following printing methods 1 to 7 is described. CI-8 manufactured by Comexi Company is used as a flexible packaging lithographic printing machine capable of installing up to 7 blanket rollers. In addition, in the following printing methods 1 to 7, the installation positions of the 7 blanket rollers are sequentially referred to as the 1st roller, the 2nd roller, the 3rd roller, the 4th roller, the 5th roller, the 6th roller, and the 7th roller from the upstream side of the traveling direction of the film to be printed. Regarding the installation position of the blanket roller not mentioned in each printing method, the roller is not pressed (impression throw-in), but by setting it at the installation position where the transfer process of the cyan, magenta, and yellow inks is not mentioned, color printing can be performed.
[0157] In the transfer process (the 1st roller and the 4th roller of the following printing methods 1, 2, 4, 5 and 7, and the 1st roller and the 6th roller of the following printing methods 3 and 6), the rubber cloth material 1 is installed on the prepared waterless planographic printing plate and the rubber cloth roller, and the active energy ray-curable ink for waterless printing is transferred to the PET film (manufactured by Polyplex, S-46, thickness 12μm) at a printing speed of 150m / min.
[0158] In the irradiation step, the ink was cured by electron beam irradiation at an acceleration voltage of 110 kV and an irradiation dose of 30 kGy to obtain a printed material. For each level, 3000 m of printing was performed.
[0159] [Printing method 1]
[0160] In the printing method 1, for the first roller, black ink 1 is provided on the ink roller, and a layer having the same Figure 1 For the 4th roller, a white ink 1 is set on the ink roller, and a waterless planographic printing plate with a pattern corresponding to the ink image 1 in the plate cylinder is set Figure 1 Waterless planographic printing plate of a pattern corresponding to the middle white image 2. The first roller and the fourth roller were roller pressed together, and the ink supply amount was adjusted so that the reflection densitometer (SpectroEye manufactured by Gretag Macbeth) of the ink solid part became 1.4.
[0161] [Printing method 2]
[0162] In the printing method 2, black ink 1 is set on the first roller, and a layer having the same Figure 1 For the fourth roller, a white ink 1 is set on the ink roller, and a waterless planographic printing plate with a pattern corresponding to the ink image 1 in the plate cylinder is set Figure 1A waterless planographic printing plate of a pattern corresponding to the white image 2 in the image is provided. In addition, a pressing roller is provided on the sixth roller. The ink supply amount is set to be the same as that of the printing method 1, and the first roller, the fourth roller, and the sixth roller are pressed together for printing.
[0163] [Printing method 3]
[0164] In the printing method 3, for the first roller, white ink 1 is provided on the ink roller, and a layer having the same Figure 1 For the sixth cylinder, black ink 1 is set on the ink roller, and a waterless planographic printing plate with a pattern corresponding to the white image 2 in the image is set on the plate cylinder. Figure 1 A waterless planographic printing plate of a pattern corresponding to the ink image 1 in the printing method 1 is provided. In addition, a pressing roller is provided for the seventh roller. The ink supply amount is set to be the same as that of the printing method 1, and the first roller, the sixth roller, and the seventh roller are pressed together for printing.
[0165] [Printing method 4]
[0166] In the printing method 4, for the first roller, black ink 1 is provided on the ink roller, and a layer having the same Figure 2 For the 4th roller, a white ink 1 is set on the ink roller, and a waterless planographic printing plate with a pattern corresponding to the ink image 3 in the plate cylinder is set on the plate cylinder. Figure 2 A waterless planographic printing plate of a pattern corresponding to the white image 4 in the figure was used. The first roller and the fourth roller were pressed together, and the ink supply amount was adjusted so that the reflection densitometer (SpectroEye manufactured by Gretag Macbeth) of the ink solid part became 1.4.
[0167] [Printing method 5]
[0168] In the printing method 5, for the first roller, black ink 1 is provided on the ink roller, and a layer having the same Figure 2 For the 4th roller, a white ink 1 is set on the ink roller, and a waterless planographic printing plate with a pattern corresponding to the ink image 3 in the plate cylinder is set on the plate cylinder. Figure 2 A waterless planographic printing plate of a pattern corresponding to the white image 4 in the image is provided. In addition, a pressing roller is provided for the third roller. The ink supply amount is set to be the same as that of the printing method 4, and the first roller, the third roller, and the fourth roller are pressed together for printing.
[0169] [Printing method 6]
[0170] In the printing method 6, for the first roller, the ink roller is provided with white ink 1, and the plate roller is provided with a Figure 2 For the sixth cylinder, black ink 1 is set on the ink roller, and a waterless planographic printing plate with a pattern corresponding to the white image 4 in the image is set on the plate cylinder. Figure 2 A waterless planographic printing plate of a pattern corresponding to the ink image 3 in the ink image 3 is provided. In addition, a pressing roller is provided for the third roller and the seventh roller. The ink supply amount is set to be the same as that of the printing method 4, and the first roller, the third roller, the sixth roller, and the seventh roller are pressed together for printing.
[0171] [Printing method 7]
[0172] In the printing method 7, for the first roller, the black ink 2 is provided on the ink roller, and the plate roller is provided with a Figure 2 For the 4th roller, a white ink 1 is set on the ink roller, and a waterless planographic printing plate with a pattern corresponding to the ink image 3 in the plate cylinder is set on the plate cylinder. Figure 2 A waterless planographic printing plate of a pattern corresponding to the white image 4 in the image is provided. In addition, a pressing roller is provided for the third roller. The ink supply amount is set to be the same as that of the printing method 4, and the first roller, the third roller, and the fourth roller are placed in the rollers and printed.
[0173] The pressure of the blanket cylinder and the impression cylinder that applies pressure to the film together with the blanket cylinder was measured by inserting a pressure-sensitive sheet (Preskel LW, manufactured by Fujifilm Corporation) between the cylinders and performing cylinder pressure in a stopped state.
[0174] <Measurement of ink printing density>
[0175] The printing density of the ink was measured using a reflection densitometer (SpectroEye manufactured by Gretag Macbeth) with the solid ink portion of the printed material as the object. The printed materials produced by printing methods 1, 2, 4, and 5 were printed on the back side, so the measurement was performed from the film surface. The printed materials produced by printing methods 3 and 6 were printed on the front side, so the measurement was performed from the ink surface.
[0176] <Point gain measurement>
[0177] The dot gain value was measured using a reflection densitometer (Spectro Eye manufactured by Gretag Macbeth) for the 50% dot portion of the printed material. The printed materials produced by printing methods 1, 2, 4, and 5 were back-printed, so the measurement was performed from the film surface. The printed materials produced by printing methods 3 and 6 were front-printed, so the measurement was performed from the ink surface. If the dot gain value is within the range of 14±4%, the dot reproducibility is good. The further away from the center 14%, the coarser or finer the dots become, and the grayscale expression is reduced.
[0178] <Peeling of the member of the pressing portion>
[0179] The presence or absence of peeling of the pressing portion member during printing and the ease of peeling of the pressing portion member from the blanket after printing were evaluated based on the following criteria.
[0180] ○: There was no peeling during printing, and the member of the pressing portion after printing was easily peeled from the blanket.
[0181] △: There was no peeling during printing, but it was difficult to peel the member of the pressing portion from the blanket after printing, and the adhesive layer also remained.
[0182] ×: The member of the pressing portion peeled off during printing.
[0183] <Measurement of surface roughness of solid parts of printed materials>
[0184] For the printed materials printed on the front side produced in printing methods 3 and 6, only the solid part was taken as the measurement object without distinguishing the ink color. 10 measurement locations were randomly extracted and the surface roughness was measured using a laser microscope (VK-X210 manufactured by Keyence Co., Ltd.) at a magnification of 20 times and a resolution of 0.1 μm.
[0185] <Gloss value of the solid part of the printed material>
[0186] For the printed matter printed on the front side produced by printing methods 3 and 6, only the solid part was taken as the measurement object without distinguishing the ink color, and 10 measurement locations were randomly selected, and the gloss value was measured at a measurement angle of 60 degrees using a precision gloss meter GM-26D (manufactured by Murakami Color Research Laboratory). A gloss value of 35 or less was considered poor, 45 or more was considered good, and 55 or more was considered extremely good.
[0187] <Measurement of Young's modulus of ink cured film>
[0188] For the printed matter printed on the front side produced in printing methods 3 and 6, for any solid part in the printed matter, a load-indentation depth graph was obtained by nanoindentation (continuous rigidity measurement method) using an ultra-microhardness tester (Nano Indenter XP, manufactured by MTS Systems). Then, the Young's modulus at an indentation depth of 0.1 μm was calculated, assuming that the Poisson's ratio of the sample was 0.4.
[0189] <Abrasion resistance of printed materials>
[0190] For the printed matter printed on the front side produced by the printing methods 3 and 6, any solid part was rubbed back and forth 20 times with the nail of the evaluator to evaluate the occurrence of scratches.
[0191] ○: No damage due to the nail was found.
[0192] ×: The ink was peeled off entirely along the trace of the nail, and the film was exposed.
[0193] [Example 1 and Comparative Examples 1 and 2]
[0194] In Example 1 and Comparative Examples 1 and 2, the pressing rollers 1, 13 and 14 based on the combination of the rubber blanket material, the member of the pressing part or the presence or absence of the pressing part, and the pattern of the pressing part shown in Table 1 were used in the corresponding order as the sixth roller for the pressing process, and printing was performed using the printing method 2. In Example 1 and Comparative Example 1 in which the pressing part was in contact with the solid part of the ink image, it was observed that the printing density of the ink was improved, and the printing density improvement effect was greater than the effect of the pressing of the pressing roller of the rubber blanket material in Comparative Example 2. Comparing Example 1 in which the solid area ratio relative to the ink image was 100% and Comparative Example 1 in which the solid area ratio relative to the ink image was 78%, in Example 1, there was no thickening of the ink dots, and the dot gain was suppressed to a small level. In Example 1 in which the pressing part was patterned in a manner that selectively contacted only the ink solid part, it was observed that the thickening of the dots was suppressed and the printing density of only the ink solid part was selectively improved. The results are shown in Tables 2 and 3.
[0195] [Comparative Example 3]
[0196] Compared with the printing method 2 (Example 1), the sixth roller for the pressing step was not pressed, and printing was performed by the printing method 1. Compared with Example 1, the roller pressing for the pressing step was not performed, so there was no smoothing effect on the printed matter. The results are shown in Table 3.
[0197] [Examples 2 to 4]
[0198] In Examples 2 to 4, pressing rollers 2 to 4 based on the combination of the rubber blanket material, the components of the pressing portion, and the pattern of the pressing portion shown in Table 1 are used in the corresponding order as the pressing process of the sixth roller, and printing is performed using printing method 2. That is, the rubber blanket material is changed, and the other aspects are the same as Example 1. The pressing portion is selectively patterned only in the solid ink portion, and in any of the examples, the effect of suppressing the thickening of the dots and selectively improving the printing density of only the solid ink portion is observed. In addition, as the resilience of the compression characteristics of the rubber blanket increases, the printing density tends to increase. On the other hand, although the pressing portion is not patterned in a manner that contacts the ink dot portion, the more highly compressible the rubber blanket is, the stronger the contact with the dot portion is, so there is a tendency for the dot gain to increase. The results are shown in Table 2.
[0199] [Examples 5 to 8]
[0200] In Examples 5 to 8, the pressing rollers 5 to 8 based on the combination of the rubber material, the member of the pressing part, and the pattern of the pressing part shown in Table 1 were used in the corresponding order as the pressing process of the sixth roller, and printing was performed using the printing method 2. That is, the type of the member of the pressing part was changed, and the other aspects were the same as Example 1. The pressing part was patterned in a manner that selectively contacted only the solid part of the ink, and in any of the examples, the effect of suppressing the coarsening of the dots and selectively improving the printing density of only the solid part of the ink was observed. In particular, the smaller the surface roughness Ra, the higher the printing density improvement effect brought about by smoothing. In addition, when comparing with the same degree of surface roughness, by setting the surface free energy of the top surface of the pressing part to 36mN / m or more, the ink adheres to the pressing part side, and the printing density improvement effect can be obtained more efficiently (comparison between Example 5 and Example 6). In addition, by setting the surface free energy to 50mN / m or less, the tendency of the concentration to decrease due to the ink being taken on the pressing part side can be suppressed (comparison between Example 1 and Example 8). The results are shown in Table 2.
[0201] [Examples 9 to 13]
[0202] According to the conditions of Example 1, only the printing pressure of the pressing roller and the impression roller was changed, and printing was performed using Printing Method 2. The pressing portion was selectively set only on the solid ink portion, and in any of the examples, the effect of suppressing the thickening of the dots and selectively improving the printing density of only the solid ink portion was observed. The higher the pressure, the higher the contact pressure between the pressing portion and the solid ink portion, so a tendency for increased printing density was observed. On the other hand, the contact pressure between the rubber blanket and the dot portion also increased, so there was also a tendency for increased dot gain. At 600 N / cm 2 When the printing density was above 1.5, there was no significant difference, and it was considered that the printing pressure was sufficient. The results are shown in Table 3.
[0203] [Example 14 and Comparative Example 4]
[0204] In Example 14 and Comparative Example 4, the pressing rollers 1 and 14 shown in Table 1 were used as the pressing process of the 7th roller in the corresponding order, and printing was performed using the printing method 3. In Example 14, which is equivalent to front printing, the pressing part is patterned in a manner that selectively contacts only the solid part of the ink, so the thickening of the dots is suppressed and the printing density of only the solid part of the ink is selectively improved. In addition, the printing density improvement effect is greater than the effect brought about by the pressing of the pressing roller of the rubber cloth material in Comparative Example 4. Compared with Comparative Example 4, the solid part of the ink of the printed material obtained in Example 14 has an Ra of 0.47μm, excellent smoothness, and the gloss of the printed material is 51, which is also good. In addition, since it is an active energy ray curing ink, the film is hard and the rub resistance is also good. The rub resistance of the printed material of Comparative Example 4 is good, but the surface roughness of the solid part is large, which is 1.04μm, and the gloss of the printed material is poor, which is 33. The results are shown in Table 4.
[0205] [Examples 15, 16 and Comparative Example 5]
[0206] In Examples 15, 16, and Comparative Example 5, the pressing rollers 9, 10, and 14 shown in Table 1 were used in the corresponding order as the pressing process of the third roller, and printing was performed using the printing method 5. Even for a complex image having many dot portions, by using a pressing roller having a properly patterned pressing portion, the effect of suppressing the thickening of the dots and selectively increasing the printing density of only the solid ink portion can be observed as in Example 15. In addition, the printing density improvement effect is greater than the effect of the pressing of the pressing roller of the rubber cloth material alone in Comparative Example 5. In addition, when Example 15 using a waterless plate printing original (component 6 of the pressing portion) as a component of the pressing portion is compared with Example 16 using a resin relief plate (component 7 of the pressing portion), in Example 15 using a waterless plate with a low surface roughness Ra, a preferred tendency that the printing density is high and the dot gain of 50% dots is close to 14% is observed. The results are shown in Table 5.
[0207] [Example 17 and Comparative Example 6]
[0208] In Example 17 and Comparative Example 6, the pressing rollers 9 and 14 shown in Table 1 were used in the corresponding order as the pressing process of the third roller, and printing was performed using the printing method 7. As in Example 15, even for a complex image having many halftone dot portions, the thickening of the halftone dots and the selective improvement of the printing density of only the ink solid portion can be observed by using a pressing roller with an appropriate pattern. In Example 17, since the pressing portion does not contact the halftone dot portion, the increase in dot gain can be suppressed compared to Comparative Example 6 in which the pressing roller of the rubber cloth material is used alone. The results are shown in Table 5.
[0209] [Comparative Example 7]
[0210] Compared with the printing method 5 (Example 15), the printing method 4 in which the third roller for the pressing process is not pressed is adopted. Compared with Example 15, the roller pressing for the pressing process is not performed, so there is no smoothing effect on the printed matter. The results are shown in Table 5.
[0211] [Examples 18, 19 and Comparative Examples 8, 9]
[0212] In Example 18, the pressing roller 12 was used for the pressing process of the third roller, and the pressing roller 9 was used for the pressing process of the seventh roller, and printing was performed by the printing method 6. In Example 19, the pressing roller 12 was used for the pressing process of the third roller, and the pressing roller 11 was used for the pressing process of the seventh roller, and printing was performed by the printing method 6. In Comparative Example 8, the pressing roller 14 was used for the pressing process of the third roller and the seventh roller, and printing was performed by the printing method 6. In Comparative Example 9, the pressing roller 13 was used for the pressing process of the third roller and the seventh roller, and printing was performed by the printing method 6. In Examples 18 and 19, for an image based on black ink, the pressing portion of the pressing roller of the seventh roller was patterned so as to selectively press only the solid portion of the ink (so as to avoid the halftone dot portion of the ink), so that the thickening of the halftone dots was suppressed and the printing density of only the solid portion of the ink was selectively improved. Moreover, in Example 19, in the pressing roller of the 7th roller, the pressing part is also patterned at the position corresponding to the white solid part, so the Ra of the solid part of the printed matter is 0.32μm, and a further smoothing effect is observed, and the gloss of the printed matter is also 60, which is very good. In addition, since it is an active energy ray curing ink, the film is hard and the wiping resistance is also good. The print of Comparative Example 8 has good wiping resistance, but the surface roughness of the solid part is large, which is 1.02μm, and the gloss of the print is poor, which is 33. The print of Comparative Example 9 smoothes the entire surface, so the gloss of the print is very good, which is 57, but the dot gain of the dot part is poor, which is 27%, and it is impossible to take into account the grayscale expression. The results are shown in Table 6.
[0213] [Reference Example 1 (Printing by intaglio front printing)]
[0214] The same image as that printed in Printing Method 6 (Examples 18, 19 and Comparative Examples 8, 9) was printed by gravure front printing. The gravure printed product of Reference Example 1 had a small surface roughness of 0.26 μm and very good glossiness, but the film was soft and therefore had insufficient scratch resistance. The results are shown in Table 6.
[0215]
[0216]
[0217] Table 4
[0218]
[0219]
[0220]
[0221] Description of Reference Numerals
[0222] 1, 3: Black ink based images
[0223] 2, 4: White ink-based images
[0224] 5: The area where the ink smoothing material is pasted
[0225] 6: Non-adhesive parts of ink-smoothing materials
[0226] D: Printing direction
[0227] N: Non-line area
[0228] B S :Ink solid part
[0229] W S : White solid part
[0230] B 50 : Ink color 50% dot area.
Claims
1. A method for producing a printed matter, comprising: a transfer step of transferring ink to a transfer surface of a printed object, and a pressing step of bringing a pressing roller into contact with the transfer surface to which the ink has been transferred, At least one of the pressing rollers has a patterned pressing portion, and through the patterned pressing portion, a portion to be smoothed and a portion not to be smoothed in the transferred surface can be selectively set, so that more than 80% of the area of the top surface of the patterned pressing portion corresponds to the solid portion transferred to the transferred surface before the pressing process, so that the smoothing effect and the grayscale expression of the dot portion can be effectively taken into account. The surface free energy of the top surface of the patterned pressing portion is greater than or equal to 36 mN / m and less than or equal to 50 mN / m.
2. The method for producing a printed matter according to claim 1, The pressure of the pressing roller having the patterned pressing portion and the impression roller facing the pressing roller having the patterned pressing portion and sandwiching the printed material is 100 N / cm 2 Above and 700N / cm 2 the following.
3. The method for producing a printed matter according to claim 1 or 2, The surface roughness Ra of the top surface of the patterned pressing portion is 0.30 μm or less.
4. The method for producing a printed matter according to claim 1 or 2, The surface roughness Rz of the top surface of the patterned pressing portion is 2.00 μm or less.
5. The method for producing a printed matter according to claim 1 or 2, The pressing cylinder having the patterned pressing portion is a cylinder on which at least one selected from an offset printing plate, a flexographic printing plate, a resin relief printing plate, and a rubber blanket is mounted.
6. The method for producing a printed matter according to claim 1 or 2, The pressing cylinder having the patterned pressing portion is a cylinder on which an offset printing plate is mounted, and the offset printing plate is a waterless plate.
7. The method for producing a printed matter according to claim 1 or 2, The pressing roller having the patterned pressing portion is a roller on which a blanket is attached, and the patterned pressing portion is an ink smoothing material attached to the blanket.
8. The method for producing a printed matter according to claim 1 or 2, The method includes a step of irradiating the ink with active energy rays after the transfer step and the pressing step.
9. The method for producing a printed matter according to claim 1 or 2, The printed object is a film.
10. The method for producing a printed matter according to claim 1 or 2, In the transfer step and the pressing step, a single impression cylinder is used which faces the cylinder for transferring ink and the pressing cylinder so as to sandwich the printed material.
11. The method for producing a printed matter according to claim 1 or 2, The value of the loss tangent, tan δ, of the ink in the pressing step at 25° C. and a measurement frequency of 10 rad / s is 1.0 or more and 4.0 or less.
12. The method for producing a printed matter according to claim 1 or 2, The transfer step is performed multiple times, and the ink used in at least the first transfer step among the multiple times is at least one of white ink and thickening ink.
13. The method for producing a printed matter according to claim 1 or 2, The method includes a pressing step performed after the pressing step using the pressing roller having the patterned pressing portion, and a pressing step performed after the transfer step using another pressing roller having the patterned pressing portion.
14. The method for producing a printed matter according to claim 8, Another transfer step is included between the pressing step performed using the pressing roller having the patterned pressing portion and the irradiation step.