A high-strength rivet-free connection method for low-ductility metal materials

Through the frictional heat generation of the cylindrical punch and the rotational movement of the tapered punch, the problem of low-strength metal materials easily generate cracks and low load-bearing capacity when there is no riveting connection is achieved, and high-strength riveting connection is achieved, which significantly improves the The load-bearing capacity of the joint.

CN115382991BActive Publication Date: 2024-11-05CHINA FAW CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211108476.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-13
Publication Date
2024-11-05
Estimated Expiration
2042-09-13

AI Technical Summary

Technical Problem

Low-stretching metal materials are prone to cracks and low load-bearing capacity when connected without riveting, resulting in connection failure.

Method used

Through the frictional heat generation of the cylindrical punch and the rotational movement of the tapered punch, the elongation of the connected plate reaches more than 12%, and the interlock value between the plates is increased to form a high-strength rivet-free connection.

Benefits of technology

High-quality connections without cracks are achieved, significantly improving the load-bearing capacity of the joints, especially for low-strength materials such as cast aluminum and cast magnesium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115382991B_ABST
    Figure CN115382991B_ABST
Patent Text Reader

Abstract

The present invention specifically relates to a high-strength rivetless connection method for low-ductility metal materials. On the basis of the traditional rivetless connection process, through appropriate process improvements, the problem of easy cracking and low load-bearing capacity of rivetless connection joints of low-ductility materials is solved, thereby ensuring high-quality connection to the vehicle body; compared with the traditional rivetless connection, the friction heat generation process between the cylindrical punch and the upper plate and the process of increasing the interlocking value between the two layers of plate by rotating the conical punch are added. The friction heat generation between the cylindrical punch and the upper plate increases the temperature of the two connected plates, the ductility is enhanced, and the elongation reaches more than 12%. For materials that are prone to cracks during rivetless connection at room temperature, this method can achieve high-quality connection without cracks; through the rotation of the conical punch, the mechanical interlocking value between the connected plates is further increased, especially for low-ductility materials, the interlocking value will be more significantly improved, thereby significantly improving the load-bearing capacity of the joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile manufacturing, and in particular to a high-strength rivet-free connection method for low-ductility metal materials. Background Art

[0002] As the global energy crisis and environmental issues become increasingly severe, countries are increasingly demanding energy conservation and emission reduction in automobiles, so lightweighting has become the main trend in automobile development. Materials such as aluminum alloys and magnesium alloys have become the main force in the field of lightweight automotive materials due to their low density, high specific strength and good corrosion resistance.

[0003] As the proportion of light alloys such as aluminum and magnesium in automobile bodies gradually increases, traditional spot welding technology can no longer meet the connection requirements of aluminum and magnesium alloys with steel materials. As a result, mechanical connection methods such as self-piercing riveting, hot-melt self-tapping connection, and rivetless connection are increasingly widely used. Among them, rivetless connection does not require the introduction of connection elements and has lower connection costs, which can further increase the lightweight effect of the vehicle body. It has currently become the main connection method for non-critical load-bearing parts in the vehicle body (such as engine hoods, back doors, etc.). However, due to the process characteristics of rivetless connection, the deformation of the connected material is large during joint formation, and the ductility of the connected parts is required to be high, and the elongation must reach more than 12%, otherwise obvious cracks will occur in the connection area, resulting in connection failure; for some aluminum and magnesium alloys that are currently widely used, especially cast aluminum and cast magnesium alloy materials, their elongation is often less than 8%, resulting in obvious cracks in the neck and bottom areas of the connection joint when rivetless connection is performed, and the joint self-locking value is very small, the joint load-bearing capacity is extremely low, and the connection fails. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the prior art that rivetless connection joints of low ductility materials are prone to cracks and have too low bearing capacity, thereby providing a high-strength rivetless connection method for low ductility metal materials.

[0005] A high-strength rivet-free connection method for low-ductility metal materials comprises the following steps:

[0006] Step 1: Place the connected upper plate and the connected lower plate on the die, and apply downward pressure through the blank holder to firmly press the connected upper plate and the connected lower plate between the die and the blank holder;

[0007] Step 2: The cylindrical punch moves downward until it contacts the upper plate of the connected plate. At this time, the cylindrical punch rotates at a certain speed, and the cylindrical punch and the upper plate of the connected plate move relative to each other. The friction heat generated increases the temperature of the upper plate and the lower plate of the connected plate until the elongation of the connected upper plate and the connected lower plate reaches the required requirement.

[0008] Step 3: After the elongation of the connected upper plate and the connected lower plate reaches the required requirement, the cylindrical punch stops rotating and moves downward at a certain speed, so that the upper plate of the connected plate and the lower plate of the connected plate are plastically deformed and filled in the pit of the die. As the punch continues to move downward, the upper plate of the connected plate begins to move sideways, so that the upper plate of the connecting plate and the lower plate of the connected plate are interlocked;

[0009] Step 4: When the cavity of the die is completely filled with the upper plate and the lower plate of the connected plate, the cylindrical punch stops moving downward, and after the cylindrical punch is kept at rest for a certain period of time, the cylindrical punch moves upward and leaves the connection area between the upper plate and the lower plate of the connected plate;

[0010] Step 5: Replace the cylindrical punch with a conical punch, and insert the conical punch into the pit of the die. At this time, rotate the conical punch around the axis of the die at a certain speed, and apply a certain lateral force to the conical punch to move the upper plate of the connected plate further to the side until the interlocking value between the upper plate of the connected plate and the lower plate of the connected plate meets the requirements;

[0011] Step 6: When the interlocking value meets the requirements, the conical punch stops rotating and then moves upward, leaving the connection area between the upper plate of the connecting plate and the lower plate of the connected plate. Then the blank holder moves upward and leaves the connection area, and the connection process ends.

[0012] Furthermore, the rotation speed of the cylindrical punch and the upper plate of the connected plate after contact is 10r / s to 100r / s, and the rotation time is 2s to 20s.

[0013] Furthermore, the elongation of the connected upper plate and the connected lower plate reaches more than 12% to meet the requirements.

[0014] Furthermore, the downward movement speed of the cylindrical punch after stopping rotation is 20 mm / s to 200 mm / s, and the downward riveting pressure is 0.5 kN to 5 kN.

[0015] Furthermore, the static time of the cylindrical punch is 1s to 10s.

[0016] Furthermore, the cone angle of the conical punch is 10° to 40°, and the maximum diameter of the lower end is 1 mm to 3 mm smaller than the diameter of the cylindrical punch (5).

[0017] Furthermore, the lateral force applied to the conical punch is 3 kN to 10 kN.

[0018] Furthermore, the interlocking value reaches 0.5 mm or more to meet the requirements.

[0019] Furthermore, structural adhesive is coated between the upper plate of the connected plates and the lower plate of the connected plates, and the thickness of the structural adhesive is 0.2 mm to 0.8 mm.

[0020] Furthermore, the upper plate and the lower plate of the connected plate are made of cast aluminum or cast magnesium, and the thickness thereof is 1 mm to 4 mm; the die, the pressure ring, the cylindrical punch and the conical punch are all made of steel, and the surfaces are all quenched.

[0021] The technical solution of the present invention adds a frictional heat generation process between the cylindrical punch and the upper plate and a process in which the conical punch rotates to increase the interlocking value between the two plates compared to the traditional rivetless connection; the frictional heat generation between the cylindrical punch and the upper plate can increase the temperature of the two connected plates, enhance the ductility, and achieve an elongation of more than 12%. For materials that are prone to cracks during rivetless connection at room temperature, such as cast aluminum and cast magnesium, this method can achieve high-quality connection without cracks; in addition, the mechanical interlocking value between the connected plates can be further increased by rotating the conical punch, especially for low-ductility materials such as cast aluminum and cast magnesium, the interlocking value improvement will be more obvious, thereby significantly improving the bearing capacity of the joint. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 Schematic diagram before and after connection;

[0024] Figure 2 It is the connection process diagram;

[0025] Figure 3 It is a schematic diagram of interlocking values;

[0026] Figure 4 Schematic diagram of the location of structural adhesive;

[0027] Description of reference numerals:

[0028] 1- Upper plate of the connected plate; 2- Lower plate of the connected plate; 3- Concave die;

[0029] 4- blank holder; 5- cylindrical punch; 6- conical punch;

[0030] 7-Structural adhesive; DETAILED DESCRIPTION

[0031] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0033] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0034] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0035] See also Figures 1 to 3 A high-strength rivet-free connection method for low-ductility metal materials comprises the following steps:

[0036] Step 1: Place the connected upper plate 1 and the connected lower plate 2 on the die 3, and apply downward pressure through the blank holder 4 to firmly press the connected upper plate 1 and the connected lower plate 2 between the die 3 and the blank holder 4;

[0037] Step 2: The cylindrical punch 5 moves downward until it contacts the upper plate 1 of the connected plate. At this time, the cylindrical punch 5 rotates at a certain speed, and the cylindrical punch 5 and the upper plate 1 of the connected plate move relative to each other. The friction heat generated increases the temperature of the upper plate 1 and the lower plate 2 of the connected plate until the elongation of the connected upper plate 1 and the connected lower plate 2 reaches the required requirement.

[0038] Step 3: After the elongation of the connected upper plate 1 and the connected lower plate 2 reaches the required requirement, the cylindrical punch 5 stops rotating and moves downward at a certain speed, so that the connected plate upper plate 1 and the connected plate lower plate 2 are plastically deformed and filled in the pit of the die 3. As the punch 5 continues to move downward, the connected plate upper plate 1 begins to move sideways, so that the connecting plate upper plate 1 and the connected plate lower plate 2 are interlocked;

[0039] Step 4: When the cavity of the die 3 is completely filled with the upper plate 1 of the connected plate and the lower plate 2 of the connected plate, the cylindrical punch 5 stops moving downward, and after the cylindrical punch 5 is kept stationary for a certain period of time, the cylindrical punch 5 moves upward and leaves the connection area between the upper plate 1 of the connected plate and the lower plate 2 of the connected plate;

[0040] Step 5: Replace the cylindrical punch 5 with a conical punch 6, and insert the conical punch 6 into the concave pit of the die 3. At this time, the conical punch 6 is rotated around the axis of the die 3 at a certain speed, and a certain lateral force is applied to the conical punch 6 to make the upper plate 1 of the connected plate move further to the side, so as to increase the interlocking value between the upper plate 1 of the connected plate and the lower plate 2 of the connected plate, thereby improving the connection strength of the joint, until the interlocking value between the upper plate 1 of the connected plate and the lower plate 2 of the connected plate meets the requirements;

[0041] Step six: When the interlocking value meets the requirements, the conical punch 6 stops rotating and then moves upward, leaving the connection area between the upper plate 1 of the connecting plate and the lower plate 2 of the connected plate, and then the pressure ring 4 moves upward to leave the connection area, and the connection process ends.

[0042] The rotation speed of the cylindrical punch 5 after contacting the upper plate 1 of the connected plate is 10r / s to 100r / s, and the rotation time is 2s to 20s, so as to ensure that the temperature of the upper plate 1 and the lower plate 2 of the connected plate rises to above 200°C, thereby ensuring that the elongation of the connected upper plate 1 and the connected lower plate 2 meets the requirements.

[0043] The elongation of the connected upper plate 1 and the connected lower plate 2 reaches more than 12% to meet the requirements.

[0044] The downward movement speed of the cylindrical punch 5 after stopping rotation is 20 mm / s to 200 mm / s, and the downward riveting pressure is 0.5 kN to 5 kN.

[0045] The static time of the cylindrical punch 5 is 1s to 10s, so that the temperature of the connected upper plate 1 and the connected lower plate 2 can be appropriately reduced.

[0046] The cone angle of the conical punch 6 is 10° to 40°, and the maximum diameter of the lower end thereof is 1 mm to 3 mm smaller than the diameter of the cylindrical punch 5 .

[0047] The lateral force applied to the conical punch 6 is 3 kN to 10 kN.

[0048] The interlocking value meets the requirement when it reaches 0.5 mm or more.

[0049] See also Figure 4 A structural adhesive 7 is also applied between the upper plate 1 and the lower plate 2 of the connected plate. The thickness of the structural adhesive 7 is 0.2 mm to 0.8 mm. Other process steps and process parameters are the same as when no structural adhesive is applied.

[0050] The upper plate 1 and the lower plate 2 of the connected plates are made of low-ductility materials, such as cast aluminum, cast magnesium, etc., with a thickness of 1mm to 4mm; the die 3, the pressure ring 4, the cylindrical punch 5 and the conical punch 6 are all made of steel, and the surfaces are quenched.

[0051] The difference between the present invention and the traditional rivetless connection is that the frictional heat generation process between the cylindrical punch and the upper plate and the process of increasing the interlocking value between the two plates by rotating the conical punch are added. The frictional heat generation between the cylindrical punch and the upper plate can increase the temperature of the two connected plates, enhance the ductility, and achieve an elongation of more than 12%. For materials that are prone to cracks during rivetless connection at room temperature, such as cast aluminum and cast magnesium, this method can achieve high-quality connection without cracks. In addition, the mechanical interlocking value between the connected plates can be further increased by rotating the conical punch, especially for low-ductility materials such as cast aluminum and cast magnesium, the interlocking value will be more significantly improved, thereby significantly improving the bearing capacity of the joint.

[0052] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A high-strength rivet-free connection method for low-ductility metal materials, characterized in that: The following steps are involved: Step 1: placing the connected upper plate (1) and the connected lower plate (2) on the die (3), and applying downward pressure through the blank holder (4) so ​​that the connected upper plate (1) and the connected lower plate (2) are firmly pressed between the die (3) and the blank holder (4); Step 2: The cylindrical punch (5) moves downward until the cylindrical punch (5) contacts the connected upper plate (1). At this time, the cylindrical punch (5) rotates at a certain speed, and the cylindrical punch (5) and the connected upper plate (1) move relative to each other. The friction heat generated increases the temperature of the connected upper plate (1) and the connected lower plate (2) until the elongation of the connected upper plate (1) and the connected lower plate (2) reaches the required requirement. Step 3: After the elongation of the connected upper plate (1) and the connected lower plate (2) reaches the required requirement, the cylindrical punch (5) stops rotating and moves downward at a certain speed, so that the connected upper plate (1) and the connected lower plate (2) are plastically deformed and filled into the concave pit of the die (3). As the cylindrical punch (5) continues to move downward, the connected upper plate (1) begins to move sideways, so that an interlocking is formed between the connected upper plate (1) and the connected lower plate (2); Step 4: When the cavity of the die (3) is completely filled with the connected upper plate (1) and the connected lower plate (2), the cylindrical punch (5) stops moving downwards. After the cylindrical punch (5) is kept stationary for a certain period of time, the cylindrical punch (5) moves upwards and leaves the connection area between the connected upper plate (1) and the connected lower plate (2); Step 5: Replace the cylindrical punch (5) with a conical punch (6), and insert the conical punch (6) into the concave pit of the die (3). At this time, the conical punch (6) is rotated around the axis of the die (3) at a certain speed, and a certain lateral force is applied to the conical punch (6) to make the connected upper plate (1) move further to the side until the interlocking value between the connected upper plate (1) and the connected lower plate (2) meets the requirements; Step 6: When the interlocking value meets the requirement, the conical punch (6) stops rotating and then moves upward to leave the connection area between the connected upper plate (1) and the connected lower plate (2), and then the blank holder (4) moves upward to leave the connection area, and the connection process ends.

2. The method according to claim 1, characterized in that The rotation speed of the cylindrical punch (5) and the connected upper plate (1) after contact is 10 r / s to 100 r / s, and the rotation time is 2s to 20s.

3. The method according to claim 1, characterized in that The elongation of the connected upper plate (1) and the connected lower plate (2) reaches more than 12% to meet the requirements.

4. The method according to claim 1, characterized in that: The downward movement speed of the cylindrical punch (5) after stopping rotation is 20 mm / s to 200 mm / s, and the downward riveting pressure is 0.5 kN to 5 kN.

5. The method according to claim 1, characterized in that The static time of the cylindrical punch (5) is 1 s to 10 s.

6. The method according to claim 1, characterized in that The cone angle of the conical punch (6) is 10° to 40°, and the maximum diameter of its lower end is 1 mm to 3 mm smaller than the diameter of the cylindrical punch (5).

7. The method according to claim 1, characterized in that The lateral force applied to the conical punch (6) is 3 kN to 10 kN.

8. The method according to claim 1, characterized in that The interlocking value meets the requirement when it reaches 0.5 mm or more.

9. The method according to claim 1, characterized in that: A structural adhesive (7) is also applied between the connected upper plate (1) and the connected lower plate (2), and the thickness of the structural adhesive (7) is 0.2 mm to 0.8 mm.

10. The method according to claim 1, characterized in that The connected upper plate (1) and the connected lower plate (2) are made of cast aluminum or cast magnesium, and have a thickness of 1 mm to 4 mm; the die (3), the blank holder (4), the cylindrical punch (5) and the conical punch (6) are all made of steel, and their surfaces are all quenched.