A method for vacuum brazing diamond abrasive grains with copper-based brazing filler metal
When brazing diamond tools in a vacuum furnace, ammonia gas is introduced to form a nitride protective layer, which solves the problems of diamond abrasive grains falling off and insufficient wear resistance of the brazing material, improves the wear resistance and life of the tool, and adapts to different processing requirements. .
Patent Information
- Application Number
- CN202211313152.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-10-25
AI Technical Summary
In the traditional diamond tool manufacturing process, diamond abrasive grains are easy to fall off, and the high melting point and low wear resistance of the solder lead to shortened tool life, and graphitization and oxidation problems are difficult to solve.
When brazing diamond tools in a vacuum furnace, nitrogen containing ammonia is introduced for cooling, and a nitride protective layer is formed under high temperature conditions to improve the wear resistance and hardness of the solder. Through the active elements in the copper-based solder, The combination of Cr, Ti, Ni and Al improves the wettability and mechanical properties of the solder.
It effectively avoids the shedding of diamond abrasive grains, improves the wear resistance and life of the tool, reduces thermal damage, and forms a wear-resistant nitride protective layer to adapt to different processing requirements.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of diamond tool manufacturing, and in particular relates to a manufacturing technology for brazing single-layer diamond tools. Background Art
[0002] As we all know, diamond has many excellent properties, such as high hardness, high wear resistance, low friction coefficient and excellent thermal conductivity, etc. Therefore, it is used to manufacture diamond tools for processing hard and brittle materials. However, due to the low diamond holding degree of traditional sintering and electroplating manufacturing processes, the diamond abrasive grains are easy to fall off during the use of the manufactured tools, and cause great pollution to the environment. Brazing diamond can form a chemical metallurgical bond between the brazing material and the diamond, improve the holding strength and exposure height of the diamond abrasive grains, and the brazed diamond tool has a longer life.
[0003] Brazing mostly uses Ni, Ag, Cu-based brazing materials containing active elements (such as Cr, Ti, V). Considering the diversity of diamond tool processing objects and usage occasions, the requirements for the melting point, composition, and wear resistance of brazing diamond tools are different from those of ordinary brazing materials, and have their own particularity and diversity. Currently, Ni, Ag, and Cu-based brazing materials are often used. Since Ni-based brazing materials have high wettability and wear resistance to diamond, their high melting point during brazing can easily cause greater thermal damage to diamond, thereby affecting the performance and service life of diamond tools. Since the solubility of C in diamond is very low in Ag and Cu bases, and Ag and Cu base solders have low melting points, the chemical erosion of diamond by Ag and Cu base solders is low, and the thermal damage to diamond is small. However, this also leads to poor wettability of diamond by Ag and Cu base solders. In order to improve the wettability of diamond by Ag and Cu bases, certain active elements need to be added. The solubility of Cr in Ag and Cu base alloys is very low, which leads to the delamination of CuCr or AgCr alloys or the formation of so-called pseudo alloys. Therefore, Ti element is often used as the active element. However, Ag and Cu base solders have low wear resistance. However, diamond tools will be subjected to high friction during processing. Temperature, so there are certain requirements for the melting point and wear resistance of the brazing filler metal to avoid the tool being easily worn out during the processing due to the brazing layer, resulting in excessive exposure of the diamond and falling off. By adding appropriate amounts of Ni and Al elements, the mechanical properties, high temperature properties and wettability of the brazing filler metal can be improved. Secondly, Ni element has good wettability to diamond, and Cu and Ni can be infinitely soluble in each other. In addition, the increase of Ni element in the brazing filler metal can appropriately increase the solubility of Cr. Al element has a low melting point and can form intermetallic compounds with Ni. By adding a certain amount of alloying elements to the brazing filler metal, the strength and wear resistance of the brazing filler metal can be improved, but too much alloying elements will increase the brittleness of the brazing filler metal. Therefore, the brazing filler metal selected is a Cu-based brazing filler metal with a small amount of Al, Ni, Cr, and Ti.
[0004] Considering that diamond is easy to graphitize during brazing, and Ti and Al are very easy to oxidize, a vacuum furnace is selected for brazing. In order to further improve the wear resistance of the brazing layer, surface treatment can also improve the wear resistance of the brazing layer, and can ensure that the brazing material has good toughness. After welding, the diamond tool is introduced into nitrogen containing ammonia for high-temperature nitriding. The N in it can react with Cr, Ti, and Al in the brazing material on the surface of the brazing material to form a thin layer of nitrides such as CrN, TiN, and AlN. The nitrogen introduced is not only conducive to quickly reducing the high temperature of diamond and avoiding diamond graphitization, but also forms a certain nitride protective layer on the surface of the brazing material, which can reduce the wear of the brazing material when the tool is in use. The brazing material has high toughness and plasticity inside, which can be better suitable for impact in grinding processing.
[0005] The present invention adopts a novel copper-based solder containing active elements for brazing, and then cools it in a furnace in nitrogen containing ammonia, which can improve the wear resistance of the brazing layer of the diamond tool, avoid the falling of diamond abrasive particles, and increase the life of the tool. Summary of the invention
[0006] The present invention adopts the method of introducing nitrogen containing ammonia to protect the brazing material when cooling the diamond in a vacuum furnace. At the same time, the brazing material will not be oxidized under vacuum and high temperature conditions. The introduction of nitrogen containing ammonia during cooling can promote the diamond abrasive grains to escape from the high temperature as soon as possible, avoid thermal damage to the diamond as much as possible, and promote the reaction between various metals on the surface of the brazing material and nitrogen in the ammonia, so that a wear-resistant layer of nitride is formed on the surface of the brazing layer, thereby improving the wear resistance and hardness of the tool brazing layer.
[0007] In order to improve the wettability of the brazing material to diamond, Ti and Cr are added to the brazing material. Since the temperature of diamond tools is high during processing, adding an appropriate amount of Ni element can improve the mechanical properties and high-temperature properties of the brazing material. At the same time, Ni element also has good wettability to diamond.
[0008] The present invention provides a novel method for manufacturing a brazed single-layer diamond grinding wheel, comprising the following steps:
[0009] (1) The required diamond grinding wheel matrix is prepared by machining, and the grinding wheel matrix is degreased and derusted.
[0010] (2) A copper-based solder is made of a certain mixture of Al, Cu, Ni, Cr and Ti, with an Al mass content of 5-8%, a Cr mass content of 2-3%, a Ti mass content of 8-10%, a Ni mass content of 20-30%, and the rest being Cu.
[0011] (3) A copper-based solder and a pressure-sensitive adhesive are mixed in a weight ratio of 1:2.3 to 2.8 to prepare a solder slurry.
[0012] (4) Brazing material slurry and diamond abrasive grains: The particle size of the diamond abrasive grains is 120-450 μm, and the thickness of the coated brazing material slurry is 95-125% of the average particle size of the diamond abrasive grains. After being mixed evenly, the brazing material slurry is coated and fixed on the surface of the grinding wheel substrate.
[0013] (5) A tool forming blank is manufactured in the order of a bottom layer of a diamond grinding wheel substrate, a middle layer of brazing material slurry, and an upper layer of diamond abrasive grains.
[0014] (6) Use a vacuum furnace to evacuate to a vacuum state, heat to 1020-1050°C and keep warm for 3-8 minutes, then introduce nitrogen containing ammonia and cool with the furnace, wherein the ammonia ratio is controlled at 20-50%, and the pressure in the vacuum furnace is maintained at 10-100 Pa. Finally, a nitride protective layer is formed on the brazing layer.
[0015] Beneficial effects of the present invention:
[0016] (1) The Cu-based solder used in the present invention has Cr as the active element, which avoids the graphitization of diamond caused by a large amount of Ni in the solder and reduces the thermal damage of diamond. In addition, the composition of the solder can be properly adjusted within a certain range to meet different processing requirements.
[0017] (3) The present invention adopts diamond vacuum brazing and then introduces nitrogen containing ammonia for furnace cooling, which can not only play an anti-oxidation role, but also react with the active elements Cr, Al, and Ti of the brazing layer in a high temperature environment to generate nitrides, thereby improving the surface hardness and wear resistance of the brazing layer, further protecting the brazing layer, and maintaining good toughness in the brazing layer to withstand the impact during grinding. DETAILED DESCRIPTION
[0018] Example 1
[0019] (1) 45 steel is selected as the grinding wheel matrix, and the required diamond grinding wheel matrix is prepared by machining method, and finally the grinding wheel matrix is degreased and derusted.
[0020] (2) A copper-based solder is made of a certain mixture of Al, Cu, Ni, Cr and Ti, with an Al mass content of 5%, a Cr mass content of 2%, a Ti mass content of 8%, a Ni mass content of 20%, and the rest being Cu.
[0021] (3) A copper-based solder and a pressure-sensitive adhesive are mixed in a weight ratio of 1:2.8 to prepare a solder slurry.
[0022] (4) The brazing material slurry and diamond abrasive grains are uniformly mixed and coated on the surface of the grinding wheel substrate according to the particle size of the diamond abrasive grains being 120 to 300 μm and the thickness of the coated brazing material slurry being 125% of the average particle size of the diamond abrasive grains.
[0023] (5) A tool forming blank is manufactured in the order of a bottom layer of a diamond grinding wheel substrate, a middle layer of brazing material slurry, and an upper layer of diamond abrasive grains.
[0024] (6) A vacuum furnace is used to evacuate to a vacuum state with a vacuum degree of 10-3Pa, and the mixture is heated to 1020°C and kept at this temperature for 3 minutes. During cooling, nitrogen containing ammonia is introduced and the mixture is cooled along with the furnace, wherein the ammonia ratio is controlled at 20%, and the nitrogen pressure is maintained at 10Pa. The mixture is cooled to room temperature in a nitrogen atmosphere and taken out.
[0025] The results show that the present invention uses nitrogen containing ammonia for nitriding and protection, which not only has an anti-oxidation effect, but also forms a certain nitride layer on the surface, which can have a certain wear-resistant effect.
[0026] Example 2
[0027] (1) 65Mn steel was selected as the grinding wheel matrix, the required diamond grinding wheel matrix was prepared by machining, and the grinding wheel matrix was degreased and derusted.
[0028] (2) A copper-based solder is made of a certain mixture of Al, Cu, Ni, Cr and Ti, with an Al mass content of 8%, a Cr mass content of 3%, a Ti mass content of 10%, a Ni mass content of 30%, and the rest being Cu.
[0029] (3) A copper-based solder and a pressure-sensitive adhesive are mixed in a weight ratio of 1:2.3 to prepare a solder slurry.
[0030] (4) The brazing material slurry and diamond abrasive grains are mixed evenly and coated on the surface of the grinding wheel substrate according to the particle size of the diamond abrasive grains of 300-450 μm and the thickness of the coated brazing material slurry is 95% of the average particle size of the diamond abrasive grains.
[0031] (5) A tool forming blank is manufactured in the order of a bottom layer of a diamond grinding wheel substrate, a middle layer of brazing material slurry, and an upper layer of diamond abrasive grains.
[0032] (6) A vacuum furnace is used to evacuate to a vacuum state with a vacuum degree of 10-4Pa, and the mixture is heated to 1050°C and kept at this temperature for 8 minutes. During cooling, nitrogen containing ammonia is introduced and the mixture is cooled along with the furnace, wherein the ammonia ratio is controlled at 50%, and the nitrogen pressure is maintained at 100Pa. The mixture is cooled to room temperature in a nitrogen atmosphere and taken out.
[0033] The results show that the use of Cu-based brazing filler metal containing active elements such as Cr and Ti reduces the thermal damage of diamond and forms a certain nitride layer on the surface during cooling, which can play a certain role in wear resistance.
[0034] Example 3
[0035] (1) 45 steel is selected as the grinding wheel matrix, and the required diamond grinding wheel matrix is prepared by machining method, and the grinding wheel matrix is degreased and derusted.
[0036] (2) A copper-based solder is made of a certain mixture of Al, Cu, Ni, Cr and Ti, with an Al content of 7%, a Cr content of 2%, a Ti content of 9%, a Ni content of 25%, and the rest being Cu.
[0037] (3) A copper-based solder and a pressure-sensitive adhesive are mixed in a weight ratio of 1:2.5 to prepare a solder slurry.
[0038] (4) The brazing material slurry and diamond abrasive grains are uniformly mixed and coated on the surface of the grinding wheel substrate according to the particle size of the diamond abrasive grains being 200 to 300 μm and the thickness of the coated brazing material slurry being 100% of the average particle size of the diamond abrasive grains.
[0039] (5) A tool forming blank is manufactured in the order of a bottom layer of a diamond grinding wheel substrate, a middle layer of brazing material slurry, and an upper layer of diamond abrasive grains.
[0040] (6) Use a vacuum furnace to evacuate to a vacuum state with a vacuum degree of 10-3Pa, heat to 1030°C and keep warm for 5 minutes, introduce nitrogen containing ammonia while cooling, and cool with the furnace, wherein the ammonia ratio is controlled at 30%, maintain the vacuum furnace pressure at 50Pa, cool to room temperature in a nitrogen atmosphere and take out.
[0041] The results show that the present invention adopts nitrogen protection containing ammonia in the vacuum furnace, which not only has the effect of anti-oxidation, but also forms a certain nitride layer on the surface, which can play a certain wear-resistant role.
[0042] Example 4
[0043] (1) The required diamond grinding wheel matrix is prepared by machining, and the grinding wheel matrix is degreased and derusted.
[0044] (2) A copper-based solder is made of a certain mixture of Al, Cu, Ni, Cr and Ti, with an Al content of 7%, a Cr content of 3%, a Ti content of 9%, a Ni content of 27%, and the rest being Cu.
[0045] (3) A copper-based solder and a pressure-sensitive adhesive are mixed in a weight ratio of 1:2.5 to prepare a solder slurry.
[0046] (4) The brazing material slurry and diamond abrasive grains are uniformly mixed and coated on the surface of the grinding wheel substrate according to the particle size of the diamond abrasive grains being 120 to 350 μm and the thickness of the coated brazing material slurry being 100% of the average particle size of the diamond abrasive grains.
[0047] (5) A tool forming blank is manufactured in the order of a bottom layer of a diamond grinding wheel substrate, a middle layer of brazing material slurry, and an upper layer of diamond abrasive grains.
[0048] (6) A vacuum furnace is used to evacuate to a vacuum state with a vacuum degree of 10-3Pa, and the mixture is heated to 1040°C and kept at this temperature for 7 minutes. During cooling, nitrogen containing ammonia is introduced and the mixture is cooled along with the furnace, wherein the ammonia ratio is controlled at 40%, and the nitrogen pressure is maintained at 60Pa. The mixture is cooled to room temperature in a nitrogen atmosphere and taken out.
[0049] The results show that under high temperature environment, N in ammonia can react with the active elements Cr, Ti, and Al in the brazing filler metal to generate nitrides, which further protect the brazing layer and improve the surface wear resistance and hardness of the brazing layer.
Claims
1. A method for vacuum brazing diamond abrasive grains with copper-based brazing filler metal, characterized in that: The method comprises the following process steps: Step 1: Preparation of grinding wheel matrix: Prepare the required diamond grinding wheel matrix by machining method, and remove oil and rust from the grinding wheel matrix; Step 2, preparation of solder: using a certain amount of Al, Cu, Ni, Cr, Ti mixed to make a copper-based solder, wherein the mass content of Al is 5-8%, the mass content of Cr is 2-3%, the mass content of Ti is 8-10%, the mass content of Ni is 20-30%, and the rest is Cu; Step 3, preparation of solder slurry: copper-based solder and pressure-sensitive adhesive are mixed in a certain weight ratio to prepare solder slurry, wherein the copper-based solder and pressure-sensitive adhesive are mixed uniformly in a weight ratio of 1:2.3-2.7; Step 4: Coating: The brazing material slurry and diamond abrasive grains are mixed evenly in a certain proportion and coated and fixed on the surface of the grinding wheel substrate; Step 5, manufacturing a tool forming blank in the order of a bottom layer of a diamond grinding wheel substrate, a middle layer of solder slurry, and an upper layer of diamond abrasive grains; Step 6: Use a vacuum furnace to evacuate to a vacuum state, heat the tool-formed blank to a certain brazing temperature and perform heat-insulating brazing, then introduce nitrogen containing ammonia to perform surface treatment on the weldment and cool it with the furnace, wherein the ammonia ratio is controlled at 20-50%, and the air pressure in the vacuum furnace is maintained at 10-100 Pa.
2. The method for vacuum brazing diamond abrasive grains with a copper-based brazing filler metal according to claim 1, characterized in that: The particle size of the diamond abrasive grains is 120-450 μm, and the thickness of the coated solder slurry is 95-125% of the average particle size of the diamond abrasive grains.
3. The method for vacuum brazing diamond abrasive grains with a copper-based brazing filler metal according to claim 1, characterized in that The vacuum state has a vacuum degree of 10 -3 ~10 -4 Pa.
4. The method for vacuum brazing diamond abrasive grains with a copper-based brazing filler metal according to claim 1, characterized in that The brazing temperature is 1020-1050°C, and the heat preservation time is 3-8 minutes.