A multi-groove grinding wheel for chamfering LCD ultra-thin screen glass and its preparation method

By designing a multi-trench grinding wheel, using the wear resistance of cobalt powder, iron powder and other materials and the polishing effect of magnesium oxide, the problem of uneven edges and collapse in the chamfering of LCD ultra-thin screen glass is solved, and the glass quality is improved rate and processing efficiency.

CN115519483BActive Publication Date: 2024-11-26QINGDAO SHINHAN DIAMOND INDUSTRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211149663.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-21
Publication Date
2024-11-26
Estimated Expiration
2042-09-21

AI Technical Summary

Technical Problem

The existing LCD ultra-thin screen glass chamfering processing has uneven edges, smooth or acute angle defects, resulting in low processing efficiency, low yield and panel fragmentation.

Method used

Using a multi-trench grinding wheel, the abrasive layer is made of mixed sintering of diamond and binder. The binder contains skeleton materials such as cobalt powder and iron powder to increase wear resistance and achieve polishing effect through magnesium oxide. The multi-trench structure is designed to reduce Cracking and increasing glass yield.

Benefits of technology

It improves the service life and blade-out ability of the grinding wheel, reduces glass breakage caused by collapse, improves the yield and processing efficiency of the glass, extends the service life of the grinding wheel, and reduces production and replacement costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115519483B_ABST
    Figure CN115519483B_ABST
Patent Text Reader

Abstract

The invention discloses a multi-groove grinding wheel for chamfering ultra-thin screen glass of LCD and a preparation method thereof, including a grinding wheel matrix and an abrasive layer, wherein the abrasive layer is sintered after mixing diamond and a binder, wherein the mass ratio of the diamond to the binder is 1:13, and the binder includes the following components in parts by weight: 8-15 parts of copper powder, 10-30 parts of tin-copper alloy powder, 5-10 parts of tin powder, 5-10 parts of tungsten disulfide powder, 8-25 parts of iron powder, 15-40 parts of cobalt powder, 2-4 parts of magnesium oxide powder, 1 part of other additives R2, and the specific components of the additive R2 include 2-4 parts of silicon powder, 0.5-1.5 parts of manganese powder, and 0.5-1 parts of rhenium powder. The grinding wheel of the present invention increases the service life of the grinding wheel; can more quickly ensure the blade and sharpness of the diamond, and improve production efficiency; reduces the glass shattering caused by the collapse, and improves the glass yield rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ultra-thin screen glass precision processing, in particular to a multi-groove grinding wheel for chamfering LCD ultra-thin screen glass and a preparation method thereof. Background Art

[0002] The ultra-thin LCD screens used now are actually thin-film silicon transistor liquid crystal displays (TFT-LCD) formed in 1993. After 2004, LCD has been in a stage of continuous prosperity and rapid development, and the products are developing towards ultra-thin and high-definition. Glass substrates are the key basic materials for LCD displays. They are mainly used for TFT processes and carriers of CF (Color Film) devices, so they are called glass substrates. That is, related circuits and processes are processed on the glass surface. The LCD display screen belongs to a sandwich structure with liquid crystal molecules clamped inside. Therefore, the glass substrate needs to meet special property requirements, including transparency, flatness, heat resistance, non-conductivity, high strength, etc.

[0003] The CF glass substrates and TFT glass used in the LCD ultra-thin screen glass industry have defects such as uneven edges, smooth edges or sharp angles after the substrates are cut by the guide wheel. In order to avoid these defects affecting subsequent processes, it is necessary to grind and chamfer the four sides of the cut glass substrates. Therefore, the LCD ultra-thin screen glass chamfering grinding wheel has become an indispensable and important process in the entire LCD panel processing process.

[0004] The TFT substrate glass used in LCD screen panels is thin, about 0.2 to 0.25 mm thick, and very brittle. Therefore, grinding it is technically difficult, requiring higher dimensional accuracy and surface edge quality, and it is easy to break during grinding, especially when processing its edges and corners, which is prone to chipping and then causing the panel to break, thus making the entire LCD panel glass scrapped. The existing chamfering grinding wheel has a low yield, low processing efficiency, large chipping, and scratches after processing, which are common problems faced by LCD ultra-thin screen glass processing. Summary of the invention

[0005] In order to overcome the above problems existing in the prior art, the present invention provides a multi-groove grinding wheel for chamfering LCD ultra-thin screen glass and a preparation method thereof.

[0006] The technical solution adopted by the present invention to solve the technical problem is: a multi-groove grinding wheel for chamfering LCD ultra-thin screen glass, comprising a grinding wheel base and an abrasive layer, wherein the abrasive layer is formed by sintering a mixture of diamond and a binder, wherein the mass ratio of the diamond to the binder is 1:13, and the binder comprises the following components in parts by weight: 8-15 parts of copper powder, 10-30 parts of tin-copper alloy powder, 5-10 parts of tin powder, 5-10 parts of tungsten disulfide powder, 8-25 parts of iron powder, 15-40 parts of cobalt powder, 2-4 parts of magnesium oxide powder, and 1 part of other additives R2.

[0007] The multi-groove grinding wheel for chamfering LCD ultra-thin screen glass has a diamond particle size of 40-50 μm or 20-30 μm.

[0008] The above-mentioned multi-groove grinding wheel for chamfering LCD ultra-thin screen glass has a diameter of 145-455 mm, a ring width of 3-10 mm, and a grinding wheel height of 20-40 mm.

[0009] The above-mentioned multi-groove grinding wheel for chamfering LCD ultra-thin screen glass has two different types of grooves arranged on the surface of the abrasive layer.

[0010] In the above-mentioned multi-groove grinding wheel for chamfering LCD ultra-thin screen glass, the specific components of the additive R2 include 2-4 parts of silicon powder, 0.5-1.5 parts of manganese powder, and 0.5-1 part of rhenium powder.

[0011] The above-mentioned method for preparing a multi-groove grinding wheel for chamfering LCD ultra-thin screen glass comprises the following steps:

[0012] Step 1, pre-treating the diamond, weighing the treated diamond and the binder in a ratio of 1:13, putting the weighed diamond and the binder into a mixing barrel, stirring and mixing for 6 hours, and vibrating and sieving to obtain a mixture;

[0013] Step 2, adding zinc stearate powder to the mixture obtained in step 1;

[0014] Step 3: weigh the mixture obtained in step 2, put it into a steel mold according to the molding requirements, and use a cold press to press 220-280kg / cm 2 Cold pressing 15-50s;

[0015] Step 4, the pressed mixture is put into a sintering furnace in a closed mold consisting of upper and lower pressure heads and front and rear baffles, and sintered at a temperature of 785°C to 850°C for 75-120 minutes;

[0016] Step 5, bonding the qualified product obtained in step 4 after measuring the relevant physical property data to the grinding wheel base to obtain a semi-finished grinding wheel;

[0017] Step 6: Design the electrode according to the groove shape required by the customer, discharge and repair the groove shape, and finally obtain the finished grinding wheel.

[0018] In the above-mentioned method for preparing a multi-groove grinding wheel for chamfering LCD ultra-thin screen glass, mold positioning is used in step 4, and the mold space is 1.08 times the height of the finished grinding wheel.

[0019] In the above-mentioned method for preparing a multi-groove grinding wheel for chamfering LCD ultra-thin screen glass, the sintering temperature in step 4 is 785° C. to 820° C., and the sintering time is 75-95 min.

[0020] In the above-mentioned method for preparing a multi-groove grinding wheel for chamfering LCD ultra-thin screen glass, the process of treating the diamond in step 1 is: applying paraffin wax to the surface of the diamond to form a uniform paraffin wax covering layer on the surface of the diamond.

[0021] The beneficial effects of the present invention are:

[0022] 1. Bonding agent for grinding wheel of the present invention

[0023] a) Through the use of cobalt powder, iron powder and other skeleton materials, the binder has excellent wear resistance and the service life of the grinding wheel is increased;

[0024] b) In combination with other additives R2, it can better improve the cutting ability while ensuring the life span, can ensure the cutting and sharpness of the diamond faster, and improve production efficiency;

[0025] c) The addition of magnesium oxide can achieve an excellent polishing effect, remove the tiny chips produced during the cutting and chamfering process of the wheel, reduce the glass breakage caused by the chips, and improve the glass yield.

[0026] 2. The abrasive layer of the present invention can be up to 40 mm high, and a grinding wheel can be distributed with up to 20 grooves. The increase in the grinding wheel height and the number of grooves reduces the time for grinding wheel installation. The multiple grooves increase the service life of the grinding wheel during use, while saving the loss of the production substrate and mold. This greatly shortens the time and replacement cost of grinding wheel production and LCD glass processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0028] Figure 1 It is a schematic diagram of the present invention;

[0029] Figure 2 This is a schematic diagram of Embodiment 5 of the present invention;

[0030] Figure 3 For the present invention Figure 2Enlarged view of part A;

[0031] Figure 4 For the present invention Figure 3 Schematic diagram of the groove in part B;

[0032] Figure 5 For the present invention Figure 3 Schematic diagram of the groove in part C.

[0033] Among them, 1. abrasive layer, 2. grinding wheel base, D is the diameter of the abrasive layer, X is the ring width of the abrasive layer, and T is the height of the grinding wheel. DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0035] This embodiment discloses a multi-groove grinding wheel for chamfering LCD ultra-thin screen glass. Figure 1 As shown in FIG. 1 , D is the diameter of the abrasive layer, which is 145-455 mm, X is the ring width of the abrasive layer, which is 3-10 mm, and T is the height of the grinding wheel, which is 20-40 mm. The structure of the grinding wheel prepared in the following embodiment is as follows: Figure 1 As shown, they are composed of two parts: a grinding wheel base 2 and an abrasive layer 1.

[0036] In the following embodiments, the abrasive layer 1 is formed by mixing diamond and a binder and then sintering. The difference lies in the specific components and component contents of the binder. The metal powder is provided by Japanese manufacturers such as Fukuda Metal / Umicore / BASF, and the diamond is purchased from South Korea's Iljin / USA DI. The particle size can be selected from 40-50um and 20-30um.

[0037] [Example 1]

[0038] In this embodiment, the binder includes the following components by weight: 10 parts of copper powder, 22 parts of tin-copper alloy powder, 5 parts of tin powder, 8 parts of tungsten disulfide powder, 15 parts of iron powder, 36 parts of cobalt powder, 3 parts of magnesium oxide powder, and 1 part of other additives R2. In this embodiment, the diamond particle size is 40-50 μm.

[0039] The specific preparation method is:

[0040] Step 1, paraffin is applied to the surface of the diamond to form a uniform paraffin covering layer on the surface of the diamond, the treated diamond and the binder are weighed in a ratio of 1:13, the weighed diamond and the binder are put into a mixing barrel, stirred and mixed for 6 hours, and vibrated and sieved through a 100-mesh vibrating screen to obtain a mixture;

[0041] Step 2, adding zinc stearate powder to the mixture obtained in step 1;

[0042] Step 3: weigh the mixture obtained in step 2, put it into a steel mold according to the molding requirements, and press it with a cold press at 250kg / cm 2 Cold pressing 35s;

[0043] Step 4, the pressed mixture is put into a sintering furnace in a closed mold consisting of upper and lower pressing heads and front and rear baffles, and sintered at 795°C for 105 minutes;

[0044] Step 5, bonding the qualified product obtained in step 4 after measuring the relevant physical property data to the grinding wheel base to obtain a semi-finished grinding wheel;

[0045] Step 6, using GC / WA grinding wheel for grinding and graphite electrode for discharge process for groove processing, after the discharge is completed, the grinding wheel is completed.

[0046] [Example 2]

[0047] In this embodiment, the binder includes the following components by weight: 12 parts of copper powder, 20 parts of tin-copper alloy powder, 7 parts of tin powder, 5 parts of tungsten disulfide powder, 12 parts of iron powder, 39 parts of cobalt powder, 4 parts of magnesium oxide powder, and 1 part of other additives R2. In this embodiment, the diamond particle size is 20-30 μm.

[0048] The specific preparation method is:

[0049] Step 1, paraffin is applied to the surface of the diamond to form a uniform paraffin covering layer on the surface of the diamond, the treated diamond and the binder are weighed in a ratio of 1:13, the weighed diamond and the binder are put into a mixing barrel, stirred and mixed for 6 hours, and vibrated and sieved through a 100-mesh vibrating screen to obtain a mixture;

[0050] Step 2, adding zinc stearate powder to the mixture obtained in step 1;

[0051] Step 3: weigh the mixture obtained in step 2, put it into a steel mold according to the molding requirements, and press it with a cold press at 250kg / cm 2 Cold pressing 35s;

[0052] Step 4, the pressed mixture is put into a sintering furnace in a closed mold consisting of upper and lower pressing heads and front and rear baffles, and sintered at 795°C for 105 minutes;

[0053] Step 5, bonding the qualified product obtained in step 4 after measuring the relevant physical property data to the grinding wheel base to obtain a semi-finished grinding wheel;

[0054] Step 6, using GC / WA grinding wheel for grinding and graphite electrode for discharge process for groove processing, after the discharge is completed, the grinding wheel is completed.

[0055] [Example 3]

[0056] In this embodiment, the binder includes the following components by weight: 10 parts of copper powder, 25 parts of tin-copper alloy powder, 5 parts of tin powder, 6 parts of tungsten disulfide powder, 12 parts of iron powder, 38 parts of cobalt powder, 3 parts of magnesium oxide powder, and 1 part of other additives R2. In this embodiment, the diamond particle size is 40-50 μm.

[0057] The specific preparation method is:

[0058] Step 1, paraffin is applied to the surface of the diamond to form a uniform paraffin covering layer on the surface of the diamond, the treated diamond and the binder are weighed in a ratio of 1:13, the weighed diamond and the binder are put into a mixing barrel, stirred and mixed for 6 hours, and vibrated and sieved through a 100-mesh vibrating screen to obtain a mixture;

[0059] Step 2, adding zinc stearate powder to the mixture obtained in step 1;

[0060] Step 3: weigh the mixture obtained in step 2, put it into a steel mold according to the molding requirements, and press it with a cold press at 250kg / cm 2 Cold pressing 35s;

[0061] Step 4, the pressed mixture is put into a sintering furnace in a closed mold consisting of upper and lower pressing heads and front and rear baffles, and sintered at 795°C for 105 minutes;

[0062] Step 5, bonding the qualified product obtained in step 4 after measuring the relevant physical property data to the grinding wheel base to obtain a semi-finished grinding wheel;

[0063] Step 6, using GC / WA grinding wheel for grinding and graphite electrode for discharge process for groove processing, after the discharge is completed, the grinding wheel is completed.

[0064] [Example 4]

[0065] In this embodiment, the binder includes the following components by weight: 15 parts of copper powder, 18 parts of tin-copper alloy powder, 9 parts of tin powder, 5 parts of tungsten disulfide powder, 8 parts of iron powder, 40 parts of cobalt powder, 4 parts of magnesium oxide powder, and 1 part of other additives R2. In this embodiment, the diamond particle size is 20-30 μm.

[0066] The specific preparation method is:

[0067] Step 1, paraffin is applied to the surface of the diamond to form a uniform paraffin covering layer on the surface of the diamond, the treated diamond and the binder are weighed in a ratio of 1:13, the weighed diamond and the binder are put into a mixing barrel, stirred and mixed for 6 hours, and vibrated and sieved through a 100-mesh vibrating screen to obtain a mixture;

[0068] Step 2, adding zinc stearate powder to the mixture obtained in step 1;

[0069] Step 3: weigh the mixture obtained in step 2, put it into a steel mold according to the molding requirements, and press it with a cold press at 250kg / cm 2 Cold pressing 35s;

[0070] Step 4, the pressed mixture is put into a sintering furnace in a closed mold consisting of upper and lower pressing heads and front and rear baffles, and sintered at 795°C for 105 minutes;

[0071] Step 5, bonding the qualified product obtained in step 4 after measuring the relevant physical property data to the grinding wheel base to obtain a semi-finished grinding wheel;

[0072] Step 6, using GC / WA grinding wheel for grinding and graphite electrode for discharge process for groove processing, after the discharge is completed, the grinding wheel is completed.

[0073] The grinding wheels obtained in Examples 1-4 were tested, and the experimental data obtained are shown in the following table:

[0074] Diamond grain size Grinding wheel speed RPM Grinding allowance μm Processing speed Single groove life Yield 40 / 50μm 4200 138 2200 108 99% 20 / 30μm 2200 60 1700 110 100% 40 / 50μm 4000 130 1700 120 100% 20 / 30μm 2000 90 1100 130 100%

[0075] It can be seen from the table that the grinding wheel produced by this formula and preparation method can effectively reduce the glass breakage caused by chipping, and the glass yield can reach 100%, effectively improving the processing efficiency.

[0076] In order to increase the long-term use of a single grinding wheel and reduce the replacement frequency, the height of the abrasive layer is increased as much as possible during the design, and more grooves (7 to 20 grooves) are formed and distributed on the outer diameter of the grinding wheel. In order to ensure the uniformity of the abrasive layer, the grinding wheel controls the pressing by positioning during the cold pressing and sintering process to ensure the uniformity of the height of the abrasive layer, thereby ensuring the similar grinding performance and life of the upper and lower grooves of the abrasive layer.

[0077] [Example 5]

[0078] In order to improve the processing efficiency, two types of diamond grains and two types of grooves can be set on one grinding wheel, so that the same grinding wheel can process different types of glass at the same time. The specific structure of the grinding wheel is as follows: Figure 2-3 As shown, the abrasive layer includes two parts, B and C. The binders of B and C include the following parts by mass: 15 parts of copper powder, 18 parts of tin-copper alloy powder, 9 parts of tin powder, 5 parts of tungsten disulfide powder, 8 parts of iron powder, 40 parts of cobalt powder, 4 parts of magnesium oxide powder, and 1 part of other additives R2. The diamond particle size used in part B is 40-50 μm, and the diamond particle size used in part C is 20-30 μm. The groove bottom widths of parts B and C are different, wherein the groove of part B is as follows: Figure 4As shown, the depth is 3-5mm, the bottom width is 3-6mm, the top angle is 40-60°, and the groove of part C is as follows Figure 5 As shown, the depth is 3-5mm, the bottom width is 1.5-3mm, and the top angle is 40-60°. The specific preparation method is as follows:

[0079] Step 1, paraffin is applied to the surface of diamond with a thickness of 40-50 μm to form a uniform paraffin covering layer on the surface of the diamond, the treated diamond and the binder are weighed in a ratio of 1:13, the weighed diamond and the binder are put into a mixing barrel, stirred and mixed for 6 hours, and vibrated and sieved through a 100-mesh vibrating screen to obtain a mixture;

[0080] Step 2, adding zinc stearate powder to the mixture obtained in step 1;

[0081] Step 3: weigh the mixture obtained in step 2, put it into a steel mold according to the molding requirements, and press it with a cold press at 250kg / cm 2 Cold pressing 35s;

[0082] Step 4, paraffin is applied to the surface of the diamond with a thickness of 20-30 μm to form a uniform paraffin covering layer on the surface of the diamond, the treated diamond and the binder are weighed in a ratio of 1:13, the weighed diamond and the binder are put into a mixing barrel, stirred and mixed for 6 hours, and vibrated and sieved through a 100-mesh vibrating screen to obtain a mixture;

[0083] Step 5, adding zinc stearate powder to the mixture obtained in step 4;

[0084] Step 6: weigh the mixture obtained in step 5, put it into a steel mold according to the molding requirements, and press it with a cold press at 250kg / cm 2 Cold pressing 35s;

[0085] Step 7, the pressed mixture is put into a sintering furnace in a closed mold consisting of upper and lower pressing heads and front and rear baffles, and sintered at 795°C for 105 minutes;

[0086] Step 8, bonding the qualified product obtained in step 7 after measuring the relevant physical property data to the grinding wheel base to obtain a semi-finished grinding wheel;

[0087] Step 9: Use GC / WA grinding wheel for grinding and graphite electrode for discharge process to process the groove. After the discharge is completed, the grinding wheel is completed.

[0088] The above embodiments are only exemplary embodiments of the present invention and are not intended to limit the present invention. The protection scope of the present invention is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.

Claims

1. A multi-groove grinding wheel for chamfering LCD ultra-thin screen glass, comprising a grinding wheel base and an abrasive layer, wherein the abrasive layer is sintered after mixing diamond and a binder, characterized in that: The mass ratio of diamond to binder is 1:13, and the binder includes the following components by weight: 8-15 parts of copper powder, 10-30 parts of tin-copper alloy powder, 5-10 parts of tin powder, 5-10 parts of tungsten disulfide powder, 8-25 parts of iron powder, 15-40 parts of cobalt powder, 2-4 parts of magnesium oxide powder, and 1 part of other additives R2; The diamond particle size is 40-50 μm or 20-30 μm; The specific components of the additive R2 include 2-4 parts of silicon powder, 0.5-1.5 parts of manganese powder, and 0.5-1 part of rhenium powder.

2. A multi-groove grinding wheel for chamfering LCD ultra-thin screen glass according to claim 1, characterized in that: The diameter of the abrasive layer is 145-455 mm, the ring width of the abrasive layer is 3-10 mm, and the height of the grinding wheel is 20-40 mm.

3. The multi-groove grinding wheel for chamfering LCD ultra-thin screen glass according to claim 1, characterized in that: The surface of the abrasive layer is provided with two different types of grooves.

4. A method for preparing a multi-groove grinding wheel for chamfering LCD ultra-thin screen glass according to any one of claims 1 to 3, characterized in that: The steps include: Step 1, pre-treating the diamond, weighing the treated diamond and the binder in a ratio of 1:13, putting the weighed diamond and the binder into a mixing barrel, stirring and mixing for 6 hours, and vibrating and sieving to obtain a mixture; Step 2, adding zinc stearate powder to the mixture obtained in step 1; Step 3: weigh the mixture obtained in step 2, put it into a steel mold according to the molding requirements, and use a cold press to press 220-280 kg / cm 2 Cold pressing 15~50s; Step 4, the pressed mixture is put into a sintering furnace in a closed mold consisting of upper and lower pressure heads and front and rear baffles, and sintered at a temperature of 785°C to 850°C for 75-120 minutes; Step 5, bonding the qualified product obtained in step 4 after measuring the relevant physical property data to the grinding wheel base to obtain a semi-finished grinding wheel; Step 6: Design the electrode according to the groove shape required by the customer, discharge and repair the groove shape, and finally obtain the finished grinding wheel; In step 4, the mold is positioned by using a mold space that is 1.08 times the height of the finished grinding wheel; In step 4, the sintering temperature is 785°C to 820°C, and the sintering time is 75-95min; The process of treating the diamond in step 1 is: applying paraffin wax to the surface of the diamond to form a uniform paraffin wax coating on the surface of the diamond.