A low-cost 950MPa grade pickled complex phase steel and its production method
By designing the composition system of C-Mn-Mo-Nb-Ti alloy and simplifying the process, the problems of high cost of pickled high-strength steel alloys and insufficient yield tensile strength are solved, and the production of low-cost 950MPa grade pickled composite steel is achieved. It has high strength and excellent forming properties, and is suitable for automotive structural parts with high safety performance requirements.
Patent Information
- Application Number
- CN202211152820.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-09-21
AI Technical Summary
The existing pickled high-strength steel has high alloy cost and insufficient yield and tensile strength, which cannot meet the use of safety parts such as anti-collision beams that require higher strength requirements. At the same time, the production process of cold-rolled composite steel is lengthy and has high manufacturing costs, which is contrary to Automobile OEM Factory’s cost reduction concept.
Design the C-Mn-Mo-Nb-Ti alloy composition system, adopts hot-mounted hot-send continuous casting and three-stage laminar flow cooling technology, combined with hot-continuous rolling and pickling processes to form ferrite, bainite, and Martha. The microstructure of the body reduces the use of Cr and V of the precious alloy elements and simplifies the production process.
The production of low-cost 950MPa grade pickled composite steel has been achieved, with a yield strength of 720-810MPa, tensile strength of 950-1080MPa, elongation after breaking ≥12%, and a hole expansion rate of ≥65%, reducing production costs and process complexity , has great market competitiveness.
Smart Images

Figure CN115537657B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a low-cost 950MPa grade pickled complex phase steel and a production method thereof. Background Art
[0002] Climate change is a major global challenge facing mankind today. In order to actively respond to climate change, my country has proposed the goal of "carbon peak and carbon neutrality". The automobile industry is a "big head" of carbon emissions. In 2022, my country's total automobile sales are expected to reach 27.5 million vehicles. If the weight of the whole vehicle is reduced by 10%, the carbon emissions of the vehicle can be reduced by 7%. Lightweighting of automobiles has become a trend in the development of automobiles in the world. High-strength steel application technology is an important shortcut to achieve lightweighting of automobiles, and pickled high-strength steel is currently the most economical material and an important raw material for future automobiles. At present, domestic steel mills have invested a lot of energy in the research and development of cold-rolled high-strength steel, and have invested less in the research and development of pickled high-strength steel. The development of pickled high-strength steel is of great significance.
[0003] The Chinese patent document with publication number CN 113481435 A discloses a 900 MPa grade hot-rolled complex phase steel and a production method thereof, wherein the chemical composition and weight percentage are as follows: C: 0.070% to 0.158%, Si: 0.08% to 0.85%, Mn: 1.15% to 2.50%, Al: 0.10% to 0.30%, Cr: 0.10% to 0.75%, Mo: 0.08% to 0.65%, B: 0.0020% to 0.0050%, and 0.025% to 0.070% of Nb and / or 0.030% to 0.155% of V, and P is limited to ≤0.020%, S is ≤0.007%, and the balance is Fe and unavoidable impurities. The complex phase steel contains elements such as Cr and V, and the alloy cost is high. In addition, the yield strength of the complex phase steel is ≥600MPa and the tensile strength is ≥900MPa. The yield and tensile strengths are low and cannot meet the use of safety parts with higher strength requirements such as anti-collision beams.
[0004] The Chinese patent document with publication number CN 112251668 A discloses a forming enhanced complex phase steel and its preparation method, the chemical composition and weight percentage of which are: C: 0.17% to 0.21%, Si: 0.2 to 0.7%, Mn: 1.8 to 2.5%, P: ≤0.01%, S: ≤0.005%, Al: 0.4 to 0.8%, Cr: 0.1 to 0.39%, Nb: 0.02 to 0.04%; and contains at least one of the following elements: Ti: 0.01 to 0.04%, Cu: 0.03 to 0.1%; the balance is Fe. The tensile strength of the complex phase steel is greater than 980 MPa, but its production process includes cold rolling and continuous annealing processes, which are lengthy and have high manufacturing costs, which is contrary to the current cost reduction concept of automobile OEMs. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a low-cost 950MPa grade pickled complex phase steel, which has the characteristics of high strength and excellent formability. The present invention also provides a production method of the low-cost 950MPa grade pickled complex phase steel.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A low-cost 950MPa grade pickled complex phase steel, the chemical composition and mass percentage of which are: C: 0.16-0.20%, Si≤0.1%, Mn: 0.8-1.2%, P≤0.02%, S≤0.01%, Als: 0.02-0.06%, Mo: 0.8-1.0%, Nb: 0.005-0.01%, Ti: 0.06-0.12%, N≤0.006%, and the balance is Fe and unavoidable impurities.
[0008] The microstructure of the complex phase steel consists of ferrite, bainite and martensite, wherein the volume proportion of the bainite structure is 60-75%, and the volume proportion of the martensite structure is 5-10%.
[0009] The complex phase steel has a yield strength of 720-810 MPa, a tensile strength of 950-1080 MPa, an elongation after fracture of ≥12%, and a hole expansion rate of ≥65%.
[0010] The production method of the low-cost 950MPa grade pickled complex phase steel comprises smelting, continuous casting, heating, hot rolling, cooling, coiling and pickling steps;
[0011] In the continuous casting process, the continuous casting billet is hot charged and hot delivered, and the casting speed is controlled at 1.0-1.5 m / min;
[0012] In the heating process, the slab entering the furnace temperature is ≥500°C, the exiting furnace temperature is controlled at 1260-1280°C, and the total time in the furnace is ≥180min;
[0013] In the hot rolling process, the finishing rolling temperature is 890-910° C. and the finishing rolling speed is 10-15 m / s.
[0014] The cooling process adopts three-stage laminar cooling, the first stage adopts water cooling, the water cooling rate is controlled at 30-50°C / s, and the intermediate temperature is controlled at 630-750°C; the second stage adopts air cooling, the air cooling time is 3-5s; the third stage adopts water cooling to the coiling temperature, the water cooling rate is greater than 100°C / s.
[0015] In the coiling process, the coiling temperature is 510-530°C.
[0016] In the pickling process, the acid solution temperature is 75-90°C.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. Design the C-Mn-Mo-Nb-Ti alloy composition system, match the corresponding TMCP process, do not add precious alloy elements Cr and V, and successfully develop low-cost 950MPa grade pickling complex phase steel with a microstructure of ferrite, bainite and martensite, reaching a yield strength of 720-810MPa, a tensile strength of 950-1080MPa, an elongation after fracture ≥12%, and a hole expansion rate ≥65%;
[0019] 2. The hot loading and hot delivery system is adopted for the continuous casting billet off-line, which makes full use of the heat energy of the continuous casting billet itself and directly enters the hot rolling process. It can not only save the energy consumption of hot rolling production and reduce production costs, but also reduce the inventory occupancy rate, shorten the product production cycle, and improve production efficiency;
[0020] 3. Compared with the currently widely used cold-rolled plates of the same strength level, this product has a short production process, does not include cold rolling and continuous annealing processes, and further reduces the production cost, making it more competitive in the market. At the same time, it has high strength and excellent formability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The microstructure diagram of the steel coil at 1 / 4 thickness of Example 1 (1000×);
[0022] Figure 2 The microstructure diagram of the steel coil at 1 / 4 thickness of Example 2 (1000×);
[0023] Figure 3 The microstructure diagram of the steel coil at 1 / 4 thickness of Example 3 (1000×);
[0024] Figure 4 The microstructure diagram of the steel coil at 1 / 4 thickness of Example 4 (1000×);
[0025] Figure 5 The microstructure diagram of the steel coil of Example 5 at 1 / 4 of the thickness (1000×);
[0026] Figure 6 The microstructure diagram of the steel coil of Example 6 at the 1 / 4 thickness position (1000×);
[0027] Figure 7 The microstructure of the steel coil of Example 7 at 1 / 4 of the thickness (1000×);
[0028] Figure 8 This is the microstructure diagram of the steel coil of Example 8 at 1 / 4 of the thickness (1000×). DETAILED DESCRIPTION
[0029] The present invention is further described in detail below with reference to the embodiments.
[0030] A low-cost 950MPa grade pickled complex phase steel, whose chemical composition and mass percentage are: C: 0.16-0.20%, Si≤0.1%, Mn: 0.8-1.2%, P≤0.02%, S≤0.01%, Als: 0.02-0.06%, Mo: 0.8-1.0%, Nb: 0.005-0.01%, Ti: 0.06-0.12%, N≤0.006%, and the balance is Fe and unavoidable impurities. Its microstructure is composed of ferrite, bainite and martensite, of which the volume proportion of bainite is 60-75%, and the volume proportion of martensite is 5-10%; the yield strength is 720-810MPa, the tensile strength is 950-1080MPa, the elongation after fracture is ≥12%, and the hole expansion rate is ≥65%.
[0031] The production method of the above-mentioned low-cost 950MPa grade pickled complex phase steel includes smelting, continuous casting, heating, hot rolling, cooling, coiling, and pickling processes; the specific process control is as follows:
[0032] (1) Continuous casting process: The continuous casting billet is hot loaded and delivered, and the casting speed is controlled at 1.0-1.5 m / min;
[0033] (2) In the heating process, the slab entering the furnace should be ≥500°C, the exiting temperature should be controlled between 1260°C and 1280°C, and the total time in the furnace should be ≥180 min.
[0034] (3) Hot rolling process: finishing rolling temperature 890-910°C, finishing rolling speed 10-15 m / s.
[0035] (4) Cooling process: three-stage laminar cooling is adopted. The first stage adopts water cooling, the water cooling rate is controlled at 30-50℃ / s, and the intermediate temperature is controlled at 630-750℃; the second stage adopts air cooling, and the air cooling time is 3-5s; the third stage adopts water cooling to the coiling temperature, and the water cooling rate is greater than 100℃ / s.
[0036] (5) Coiling process: Coiling temperature 510-530°C.
[0037] (6) Pickling process: Use hydrochloric acid at a certain temperature to continuously remove the iron oxide scale. The acid temperature is 75-90℃.
[0038] The chemical composition mass percentages of the pickled complex phase steels of Examples 1-8 are shown in Table 1, the control parameters of each process step of the production steps are shown in Tables 2 and 3, and the mechanical properties and microstructures are shown in Table 4.
[0039] Table 1. Chemical composition mass percentage (%) of pickled complex phase steel in each embodiment
[0040]
[0041] Table 2. Parameters of continuous casting, heating and hot rolling processes in various embodiments
[0042]
[0043] Table 3. Cooling, coiling and pickling process parameters of various embodiments
[0044]
[0045] Table 4 Mechanical properties and microstructure of pickled complex phase steel in various examples
[0046]
[0047] Figure 1-Figure 8 It is shown that the pickled complex phase steel produced by the present invention has the structure of ferrite + bainite + martensite, wherein the bainite structure accounts for 60-75% by volume, the martensite structure accounts for 5-10% by volume, the yield strength is 720-810MPa, the tensile strength is 950-1080MPa, the elongation after fracture is ≥12%, and the hole expansion rate is ≥65%. The pickled complex phase steel of the present invention has the characteristics of high strength and excellent formability, and is suitable for structural parts with high safety performance requirements such as front and rear anti-collision beams and door sill beams of automobiles, and has good application prospects.
Claims
1. A low-cost 950MPa grade pickled complex phase steel, characterized in that: Its chemical composition and mass percentage are: C: 0.16-0.20%, Si≤0.090%, Mn: 0.8-1.18%, P≤0.02%, S≤0.01%, Als: 0.02-0.06%, Mo: 0.8-1.0%, Nb: 0.005-0.01%, Ti: 0.06-0.12%, N≤0.006%, the balance is Fe and unavoidable impurities; The microstructure of the complex phase steel is composed of ferrite, bainite and martensite, wherein the volume proportion of bainite is 60-75%, and the volume proportion of martensite is 5-10%; The complex phase steel has a yield strength of 720-810 MPa, a tensile strength of 950-1080 MPa, an elongation after fracture of ≥12%, and a hole expansion rate of ≥65%.
2. The method for producing low-cost 950MPa grade pickled complex phase steel according to claim 1, characterized in that: It includes smelting, continuous casting, heating, hot rolling, cooling, coiling and pickling processes; In the continuous casting process, the continuous casting billet is hot charged and hot delivered, and the casting speed is controlled at 1.0-1.5 m / min; In the heating process, the slab entering the furnace temperature is ≥500°C, the exiting furnace temperature is controlled at 1260-1280°C, and the total time in the furnace is ≥180min; The cooling process adopts three-stage laminar cooling, the first stage adopts water cooling, the water cooling rate is controlled at 30-50°C / s, and the intermediate temperature is controlled at 630-750°C; the second stage adopts air cooling, the air cooling time is 3-5s; the third stage adopts water cooling to the coiling temperature, the water cooling rate is greater than 100°C / s.
3. The method for producing low-cost 950MPa grade pickled complex phase steel according to claim 2, characterized in that: In the hot rolling process, the finishing rolling temperature is 890-910° C. and the finishing rolling speed is 10-15 m / s.
4. The method for producing low-cost 950MPa grade pickled complex phase steel according to claim 3, characterized in that: In the coiling process, the coiling temperature is 510-530°C.
5. The method for producing low-cost 950MPa grade pickled complex phase steel according to any one of claims 2 to 4, characterized in that: In the pickling process, the acid solution temperature is 75-90°C.
Citation Information
Patent Citations
Formed reinforced complex phase steel and preparation method thereof
CN112251668A
900MPa-grade hot-rolled complex-phase steel and production method thereof
CN113481435A
Ultrahigh strength hot-rolled complex phase steel plate and production method thereof
CN109023036A
Hot-rolled and acid-washed complex-phase steel with excellent surface quality and preparation method thereof
CN110306102A
1180MPa-grade high-plasticity bainite complex phase steel plate for automobile and preparation method for 1180MPa-grade high-plasticity bainite complex phase steel plate
CN110724877A