A method for pre-adjusting the melting state of mold protection slag

By pre-heating mold protection slag based on its transition and melting temperatures, the method addresses the inefficiencies in existing methods, enhancing melting speed and uniformity while reducing agglomeration and carbon contamination in the continuous casting process.

CN115555533BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD +1
View PDF 0 Cites -1 Cited by

Patent Information

Application Number
CN202211179129.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-12-03
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

Existing methods for controlling the melting rate of mold powder in the continuous casting process are inadequate to meet the higher requirements of modern steel mills, leading to issues such as agglomeration and non-uniform phase formation of the mold protection slag.

Method used

A method involving pre-heating the mold protection slag before adding it to the crystallizer, with a heating temperature determined by the transition and melting temperatures of the slag, and using a heating coil or hot air to ensure no liquid phase is present, thereby optimizing the melting process.

Benefits of technology

The method increases the melting speed of the mold protection slag by 30-40%, enhances phase uniformity, reduces agglomeration, and decreases carbon contamination in molten steel, improving the overall efficiency and effectiveness of the continuous casting process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a method for pre-adjusting the melting state of a mold protection slag. Before the mold protection slag is added to the crystallizer, the mold protection slag is heated, and the heated mold protection slag is added to the crystallizer. It is required that no liquid phase appears in the mold protection slag added to the crystallizer. The present invention increases the temperature of the mold protection slag before it enters the crystallizer, and at the same time considers the transition temperature and melting temperature of the protection slag to ensure that the protection slag will not be over-melted in the feeding rod. The energy required for the molten steel to melt the mold protection slag entering the crystallizer is reduced, the agglomeration of the protection slag is greatly improved, the initial liquid slag thickness is increased, the risk of slag rolling is reduced, the melting speed of the mold protection slag is accelerated, and the uniformity of the phase after melting is improved. At the same time, the carbonate in the mold protection slag is decomposed into carbon dioxide and oxygen during the heating process, which reduces the carbon increase of the molten steel caused by the dissolution of carbonate in the molten pool on the surface of the crystallizer, and alleviates the carbon increase effect of the protection slag.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of continuous casting, and in particular to a method for pre-adjusting the melting state of a crystallizer protective slag. Background Art

[0002] Mold powder is an important raw material in the continuous casting process of steelmaking. It has the functions of improving heat transfer, enhancing lubrication, heat preservation, preventing secondary oxidation of molten steel, and absorbing inclusions. The melting rate of the powder can be adjusted and controlled by the carbon content in the powder. At the same time, the carbon content in the powder also ensures the uniformity of the powder phase after melting and avoids the agglomeration of the powder. With the advancement of technology, steel mills have higher requirements for mold powder. The original process methods such as controlling the melting rate of the powder by the carbon content in the powder can no longer meet the needs of modern steel mills. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for pre-adjusting the melting state of the mold protection slag, so as to increase the melting speed of the mold protection slag in the crystallizer.

[0004] To achieve the above object, the present invention adopts the following technical solutions:

[0005] A method for pre-adjusting the melting state of a mold protection slag, wherein the mold protection slag is heated before being added into a crystallizer, and the heated mold protection slag is added into the crystallizer; and it is required that no liquid phase appears in the mold protection slag added into the crystallizer.

[0006] The heating temperature △T of the mold protection slag is determined according to formula (1):

[0007] △T=(1.2T 转折 +0.8T 熔化 ) / 2-300 (1)

[0008] In formula (1):

[0009] △T: Heating temperature of mold protection slag / ℃;

[0010] T 转折 : Transition temperature of mold protection slag / ℃;

[0011] T 熔化 : Melting temperature of mold protection slag / ℃;

[0012] The crystallizer protection slag heating method adopts heating coil heating, and the heating power of the heating coil is calculated according to the following formula:

[0013] P = dQ / (dt×η); (2)

[0014] In formula (2):

[0015] P: heating coil power / kW;

[0016] η: thermal efficiency, η = 80%;

[0017] dQ: Energy required for heating the mold protection slag for dt time / J;

[0018] dQ=C p m△T; (3)

[0019] In formula (3):

[0020] C p : Specific heat of mold powder / JK -1 kg -1 ;

[0021] m: weight of mold protection slag / kg;

[0022] m=ν×dt; (4)

[0023] In formula (4):

[0024] ν: feeding speed / kg s -1 .

[0025] Therefore, P = dQ / (dt × η) = [C p (ν×dt)△T] / (dt×η)=C p ν△Tη -1 .

[0026] The heating coil is installed on the feeding rod of the crystallizer protection slag feeder.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention increases the temperature of the mold protection slag before it enters the crystallizer, and at the same time considers the transition temperature and melting temperature of the protection slag, so as to ensure that the protection slag will not be over-melted in the feeding rod. The energy required for the molten steel to melt the mold protection slag entering the crystallizer is reduced, the agglomeration of the protection slag is greatly improved, the initial liquid slag thickness is increased, the risk of slag rolling is reduced, the melting speed of the mold protection slag is accelerated, and the uniformity of the phase after melting is improved.

[0029] At the same time, the carbonate in the mold protection slag is decomposed into carbon dioxide and oxygen during the heating process, which reduces the carbon increase of the molten steel caused by the dissolution of carbonate in the molten pool on the surface of the crystallizer and alleviates the carbon increase effect of the protection slag.

[0030] The invention increases the melting speed of mold protection slag by 30-40%, increases the thickness of liquid slag by 2-5 mm, eliminates the caking phenomenon of protection slag, reduces the carbon increase of molten steel by the crystallizer protection slag by 1-2 ppm, and optimizes the use effect of the protection slag. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] A method for pre-adjusting the melting state of a mold powder, comprising installing a heating coil on a feeding rod of a mold powder feeder;

[0033] Before the mold protection slag is added to the crystallizer, the mold protection slag is heated and the heated mold protection slag is added to the crystallizer; it is required that no liquid phase appears in the mold protection slag added to the crystallizer, and the heating temperature △T of the mold protection slag is determined according to the turning temperature of the mold protection slag and the melting temperature of the mold protection slag;

[0034] △T=(1.2T 转折 +0.8T 熔化 ) / 2-300 (1)

[0035] In formula (1):

[0036] △T: Heating temperature of mold protection slag / ℃;

[0037] T 转折 : Transition temperature of mold protection slag / ℃;

[0038] T 熔化 : Melting temperature of mold protection slag / ℃;

[0039] The heating power of the heating coil is calculated according to the following formula:

[0040] P = dQ / (dt×η); (2)

[0041] In formula (2):

[0042] P: Heating power of heating coil / kW;

[0043] η: thermal efficiency, η = 80%;

[0044] dQ: Energy required for heating the mold slag for dt time / J;

[0045] dQ=C p m△T; (3)

[0046] In formula (3):

[0047] C p : Specific heat of mold powder / JK -1 kg -1 ;

[0048] m: weight of mold slag / kg; m = ν × dt; (4)

[0049] In formula (4):

[0050] ν: feeding speed / kg s -1 .

[0051] From formulas (2), (3) and (4), we can get:

[0052] dQ / dt=[C p (ν×dt)△T] / dt;

[0053] P=dQ / (dt×η)=[C p (ν×dt)△T] / (dt×η)=C p ν△Tη -1 .

[0054] Example

[0055] A method for pre-adjusting the melting state of the mold powder is to install a heating coil on the feeding rod of the mold powder feeder;

[0056] The heating temperature △T of the mold protection slag is determined according to the transition temperature of the mold protection slag and the melting temperature of the slag for mold protection;

[0057] The transition temperature of the mold protection slag is 1000°C, the melting temperature of the mold protection slag is 950°C, and the feeding speed is 1.3kg / min.

[0058] Heating temperature of mold protection slag △T=(1.2T 转折 +0.8T 熔化 ) / 2-300=(1.2×1000+0.8×950) / 2-300=680°C.

[0059] The heating power of the heating coil P = dQ / (dt×η) = [C p (ν×dt)△T] / (dt×η)=C p ν△Tη -1 =1250×10 -3 ×(1.3÷60)×680×(80%) -1 =23kW.

[0060] Heating coil heating power = 23kW.

[0061] According to the above method, it is calculated that when the transition temperature of the mold protection slag is 1000℃ and the melting temperature of the slag for crystallizer protection is 950℃, the feeding speed is 1.3kg / min; the heating power of the heating coil is set to 23kW.

[0062] The heating method of the present invention is not limited to heating with a heating coil, and hot air heating can also be used.

[0063] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for pre-adjusting the melting state of mold casting slag, characterized in that: Before the mold slag is added to the crystallizer, the mold slag is heated and added to the crystallizer. It is required that no liquid phase appears in the mold slag added to the crystallizer. The heating temperature △T of the mold slag is determined according to formula (1): △T=(1.2T 转折 +0.8T 熔化 ) / 2-300 (1) In formula (1): △T: Heating temperature of mold protection slag / ℃; T 转折 : Transition temperature of mold protection slag / ℃; T 熔化 : Melting temperature of mold protection slag / ℃.

2. The method for pre-adjusting the melting state of mold protection slag according to claim 1, characterized in that: The crystallizer protection slag heating method adopts heating coil heating, and the heating power of the heating coil is calculated according to the following formula: P = dQ / (dt × η); (2) In formula (2): P: Heating power of heating coil / kW; η: thermal efficiency, η=80%; dQ: Energy required for heating the mold protection slag for dt time / J; dQ=C p m△T; (3) In formula (3): C p : Specific heat of mold powder / J / (kg·℃); m: weight of mold protection slag / kg; m = ν × dt; (4) In formula (4): ν: feeding speed / kg s -1 ; Therefore, P = dQ / (dt×η) = [C p (ν×dt)△T] / (dt×η)=C p ν△Tη -1 .

3. A method for pre-adjusting the melting state of mold protection slag according to claim 2, characterized in that: The heating coil is installed on the feeding rod of the crystallizer protection slag feeder.

4. The method for pre-adjusting the melting state of mold casting slag according to claim 1, characterized in that: The crystallizer protection slag is heated by hot air.