A polyvinylidene fluoride device with embedded pipe and preparation method thereof
The surface of the polyvinylidene fluoride material is trimmed by mechanical grinding and laser heating scanning technology, and the guide hole-paraffin-cooling-pipe technology is used to remove burrs to form a micro-nano structure surface, which solves the problem of poor water circulation in cooling equipment and improves efficiency. Cooling effect and service life.
Patent Information
- Application Number
- CN202211209895.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-09-30
AI Technical Summary
The hydrophobic surface of polyvinylidene fluoride material in cooling equipment causes poor circulation of cooling water and is prone to flooding, which affects the cooling effect.
Mechanical grinding and laser heating scanning technology are used to trim the surface of the polyvinylidene fluoride material, combined with the processing technology of guide hole-paraffin-cooling-pipeline, to form a micro-nano structure surface, improve its hydrophobic properties and remove burrs generated after drilling, to achieve a Cooling appliance design with multiple inlets and outlets.
It improves the hydrophilic and hydrophobic properties of polyvinylidene fluoride materials, enhances the water circulation and service life of cooling equipment, and reduces the impact of air liquid water on cooling objects.
Smart Images

Figure CN115556177B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cooling devices, and in particular to a polyvinylidene fluoride device with an embedded pipeline and a preparation method thereof. Background Art
[0002] Polyvinylidene fluoride (PVDF) is a highly non-reactive thermoplastic fluoropolymer and a linear semi-crystalline thermoplastic engineering plastic. It has good chemical corrosion resistance, high temperature resistance, oxidation resistance, weather resistance, radiation resistance and good chemical stability. Its applications are mainly concentrated in the fields of petrochemicals, electronics and fluorocarbon coatings. PVDF is one of the best materials for pumps, valves, pipes, pipe fittings, storage tanks and heat exchangers in the fluid handling system of petrochemical equipment as a whole or lining. It is one of the materials for chemical-resistant parts and wires and cables. It has many uses, but it has not been used in cooling equipment.
[0003] Polyvinylidene fluoride material has no hydrophilic group and has poor hydrophilicity. When it is used to carry water-related items, it is difficult to absorb the moisture of the carried items and take away the moisture. Long-term use of the material will cause flooding and other phenomena to the carried objects. If the surface of the polyvinylidene fluoride material is modified to achieve better hydrophilicity of the polyvinylidene fluoride PVDF material, its surface can be modified to meet the better hydrophilic characteristics and absorb some moisture of the carried object. Cooling equipment generally uses built-in pipes. When cooling water circulates in the built-in pipes, it is necessary to have smooth water flow. The surface with hydrophobic characteristics will have a good effect on the smooth water flow. The built-in pipes are constructed with micro-nano structures to increase their roughness, thereby showing a hydrophobic phenomenon when they come into contact with water. In terms of cooling equipment, by processing micro-nano structures, its hydrophobicity can be increased, and cooling water can be prevented from infiltrating the cooling equipment, so that after long-term use, the surface of the cooling equipment is covered with moisture to hinder the water flow, which greatly affects the objects that need to be cooled, such as wafers and substrates. Summary of the invention
[0004] The present invention adopts a new material polyvinylidene fluoride embryo disc to carry out a rational design of the pipeline, adopts a central pipeline to connect the hollow cavity, and then connects it with the embedded pipeline to realize a one-inlet and multiple-outlet cooling device; combined with the improvement in processing technology, mechanical grinding technology is adopted to polish and grind its surface. Because the surface will be damaged to a certain extent during grinding, laser heating and scanning its surface are adopted to repair the damage on the surface, so that the surface is flatter and smoother. The flat and smooth surface is beneficial to the hydrophilicity of the polyvinylidene fluoride material; the guide hole-paraffin-cooling-pipeline processing technology is adopted to solve the burr phenomenon caused by drilling, avoid the influence of burrs on later use, etc., and can realize the formation of a micro-nano structure surface on the inner wall of the pipeline, improve the hydrophobic properties of its surface, etc.
[0005] A polyvinylidene fluoride device with an embedded pipe, the device comprising: a polyvinylidene fluoride body, an embedded pipe and a central mechanism, the polyvinylidene fluoride body is a prism, the center of the prism is provided with the central mechanism, the central mechanism comprises a central pipe, the central pipe is arranged on the midline of the prism, the central pipe extends from the center of the prism to the bottom surface of the prism and passes through the bottom surface of the prism, the embedded pipe is connected to the surrounding of the central mechanism, the embedded pipe extends from the edge of the central mechanism to the edge surface of the prism, and the embedded pipe passes through the edge surface of the prism, the inner wall of the embedded pipe and the inner wall of the central mechanism are both rough surfaces, the outer surface of the polyvinylidene fluoride body is a smooth surface, and the embedded pipe and the central mechanism are through-connected.
[0006] Furthermore, the central mechanism also includes a hollow cavity, the bottom center of the hollow cavity is connected to the central pipe, and the surrounding of the hollow cavity is connected to the embedded pipe.
[0007] Furthermore, the polyvinylidene fluoride body is a regular prism.
[0008] Furthermore, the embedded pipes are all arranged on the central plane of the polyvinylidene fluoride body.
[0009] Furthermore, the number of the embedded pipes is equal to the number of facets of the prism.
[0010] Furthermore, the center point of the edge surface of the prism is on the center line of the embedded pipe.
[0011] Furthermore, the inner wall of the embedded pipe is a rough surface with a micro-nano structure.
[0012] Furthermore, the inner wall of the central mechanism is a rough surface of micro-nano structure.
[0013] Furthermore, the inner wall of the embedded pipe and the central mechanism is made of polyvinylidene fluoride body.
[0014] Furthermore, the polyvinylidene fluoride body, the embedded pipe and the central mechanism are integrally formed.
[0015] Furthermore, the diameter of the embedded pipe is not greater than 1 / 3 of the thickness of the polyvinylidene fluoride body.
[0016] Furthermore, the inscribed circle of the regular prism is selected from a regular prism of 6 inches, 8 inches or 12 inches.
[0017] A method for preparing a polyvinylidene fluoride device with an embedded pipeline, the specific steps are as follows:
[0018] Step 1: Making the round billet
[0019] A round ingot made of polyvinylidene fluoride (PVDF) is selected, placed on a cutting machine for cutting, and a cutting saw is selected to cut the round ingot into a round blank of the required thickness;
[0020] Step 2: Making prismatic embryos
[0021] Select the round blank of step 1, put it on the stage of the cutting machine, select a straight cutting saw to cut the equilateral prism, cut the equilateral prism, and then mill the surface of the equilateral prism, put it on the milling machine for milling to obtain the flatness of each surface, mill the chamfer, and then polish it. Use mechanical polishing technology and laser scanning technology to first mechanically polish the flat surface with oilstone to obtain an equilateral prism with the required smoothness, and then perform laser heating scanning on the surface to repair the micro-nano traces of surface damage, and further melt and solidify the surface to obtain a flat, smooth and undamaged surface, which is called a polyvinylidene fluoride body;
[0022] Step 3: Make the first embedded guide hole
[0023] Select the polyvinylidene fluoride body of step 2, place its first edge face on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, the buffer pad and the fixture are used to stabilize and protect the polyvinylidene fluoride body, fix the polyvinylidene fluoride body, start the drill bit at the center of the first edge face relative to the edge face, and drill the first embedded guide hole along the straight line between the center of the edge face and the center of the polyvinylidene fluoride body, and drill to the center of the polyvinylidene fluoride body;
[0024] Step 4: Make the embedded guide holes on the remaining edges
[0025] Select the polyvinylidene fluoride body of step 3, and process the embedded guide holes at the centers of the remaining edge faces according to the processing method of step 3 to form embedded guide holes that gather at the center of the polyvinylidene fluoride body and diverge from the edge faces, and drill the embedded guide holes of the polyvinylidene fluoride body;
[0026] Step 5: Make the center guide hole on the bottom surface of the PVDF body
[0027] Select the polyvinylidene fluoride body of step 4, place its top surface on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, the buffer pad and the fixture are used to stabilize and protect the polyvinylidene fluoride body, fix the polyvinylidene fluoride body, start the drill bit at the center of the top surface relative to the bottom surface, and drill along the center line of the prism to the convergence of the embedded guide holes at the center of the polyvinylidene fluoride body to obtain the interconnection between the central guide hole and the embedded guide hole. At this time, the inner wall of each processed guide hole and the central hollow cavity has many burrs, which will greatly affect the circulation of water and the long-term use of the cooling device;
[0028] Step 6: Make the first embedded pipe
[0029] Select the polyvinylidene fluoride body of step 5, place its first edge face on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, the buffer pad and the fixture are used to stabilize and protect the polyvinylidene fluoride body, fix the polyvinylidene fluoride body, and pour paraffin liquid at the first embedded guide hole to fill the first embedded guide hole. Since the temperature of the paraffin liquid is much lower than the melting point of the polyvinylidene fluoride, it will not cause serious damage to the polyvinylidene fluoride on the wall of the first embedded guide hole. Since the first embedded guide hole is a thin and long guide hole, and the thermal conductivity of the polyvinylidene fluoride body is weak, the cooling of the liquid paraffin is very slow. Therefore, some cooling gases (dry ice, nitrogen, etc.) are used for rapid cooling and solidification (using induction The cooling gas can also solidify the burrs caused by the processing of the first guide hole. Liquid paraffin can quickly solidify the burrs. Since paraffin is added as an auxiliary agent during the manufacture of the polyvinylidene fluoride material, the processed polyvinylidene fluoride material will contain a small amount of paraffin. Then, the filled paraffin can be used. According to the principle of attraction of substances, some paraffin can enter the polyvinylidene fluoride body. Then, a drill bit with a diameter 0.15-0.2mm larger than that of the drill bit for processing the guide hole is used for drilling. The drill is drilled to the confluence of the embedded guide holes at the center of the polyvinylidene fluoride body to complete the preparation of the first embedded pipeline. During the drilling process, paraffin will also play a lubricating and grinding role. When the drill bit is drilling, the inner surface of the micro-nano structure will be formed.
[0030] Step 7: Make the embedded pipes on the remaining edges
[0031] Select the polyvinylidene fluoride body of step 6, and process the embedded pipes at the center of the remaining facets according to the processing method of step 6 to form embedded pipes gathered at the center of the polyvinylidene fluoride body and diverging from the facets, and drill the embedded pipes of the polyvinylidene fluoride body;
[0032] Step 8: Make the center embedded pipe on the bottom surface of the PVDF body
[0033] Select the polyvinylidene fluoride body of step 7, place its top surface on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, the buffer pad and the fixture are used to stabilize and protect the polyvinylidene fluoride body, fix the polyvinylidene fluoride body, and pour paraffin liquid into the central guide hole, fill the central guide hole with paraffin liquid, and use some cooling gas (dry ice, nitrogen, etc.) to quickly cool and solidify (using the blowing method at the guide hole). Since paraffin is added as an auxiliary agent during the manufacture of the polyvinylidene fluoride material, the processed polyvinylidene fluoride material will contain a small amount of paraffin component, and then use the filled paraffin. The principle of attraction of substances allows some paraffin to enter the polyvinylidene fluoride body, and then use a drill bit with a diameter 0.15-0.2mm larger than the drill bit for processing the guide hole to drill to the embedded pipe confluence at the center of the polyvinylidene fluoride body to complete the preparation of the central embedded pipe;
[0034] Step 9: Detection
[0035] After the inner side of the embedded pipe was cut open, no obvious burrs were observed under a 20x magnifying glass, and after the hollow cavity was cut open, no obvious burrs were observed under a 20x magnifying glass, achieving effective use results; under a contact angle tester, the surface contact angle of the device was measured to be about 65°, and the surface contact angle of the inner wall of the embedded pipe was measured to be about 140°.
[0036] Furthermore, the specification and size of the drill bit are selected according to the required processing size.
[0037] Beneficial Effects
[0038] The present invention adopts a new material polyvinylidene fluoride embryonic disc, performs a rational design of the pipeline, adopts a central pipeline to connect the hollow cavity, and then connects with the embedded pipeline to realize a one-inlet and multiple-outlet cooling device; adopts a drilling neck smaller than 1 / 3 of the thickness of the polyvinylidene fluoride embryonic disc, and is processed and formed on the central surface of the polyvinylidene fluoride embryonic disc, adopts an integrated molding technology, realizes uniform cooling of the cooling device, uniform flushing, etc.; combined with the improvement in processing technology, adopts mechanical grinding technology to polish and grind its surface, trim its surface flatness, improve its surface energy, so as to improve its hydrophilicity, when cooling high-precision integrated circuit wafers, it can absorb as much air and liquid water as possible, reduce the influence of air and liquid water on the wafers, on the other hand, because the surface will be damaged to a certain extent during grinding, the use of laser Scan its surface with optical heating to repair the damage on its surface and make it flatter and smoother. The flat and smooth surface will be beneficial to the hydrophilicity of the polyvinylidene fluoride material and better reduce the liquid water in the air. The guide hole-paraffin-cooling-pipeline processing technology is adopted. When processing the guide hole, the drill bit will react violently with the polyvinylidene fluoride material, and burrs will appear in the drilling and grinding process. The existence of these burrs will affect the circulating water. Paraffin is used for filling, and then dry ice is used for cooling. A drill bit that is 0.15-0.2mm larger than the guide hole rotor is used for secondary drilling. The drill bit is lubricated by paraffin, and the burrs are solidified by paraffin, so the burr phenomenon caused by drilling is solved to avoid the impact of burrs in later use. This technology can be widely used in deburring, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a schematic diagram of the front structure of a polyvinylidene fluoride device with an embedded pipeline according to the present invention.
[0040] Figure 2 This is a schematic diagram of the back structure of a polyvinylidene fluoride device with an embedded pipeline according to the present invention.
[0041] Figure 3 The present invention is a schematic diagram of a cross-sectional front view of a polyvinylidene fluoride device with an embedded pipe.
[0042] Figure 4 The figure is a schematic diagram of the cross-sectional structure of a polyvinylidene fluoride device with an embedded pipe according to the present invention.
[0043] Figure 5 The figure is a schematic diagram of the central cross-sectional structure of a polyvinylidene fluoride device with an embedded pipe according to the present invention.
[0044] Figure 6 The present invention is a flow chart of the preparation process of a polyvinylidene fluoride device with an embedded pipe.
[0045] Figure 7 This is a diagram showing the hydrophilicity and hydrophobicity of a polyvinylidene fluoride device with an embedded pipe according to the present invention.
[0046] Description of the drawings: 01, top surface; 02, embedded pipe; 03, prism surface; 04, bottom surface; 05, central pipe; 11, round embryo; 12, prismatic embryo; 13, first embedded guide hole; 14, remaining embedded guide holes; 15 central guide hole; 16, first embedded pipe; 17, remaining embedded pipes; 18, central embedded pipe; 19, detection. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] In the present invention, the term "multiple" refers to two or more. "And / or": describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The character " / " generally indicates that the related objects are in an "or" relationship.
[0049] See also Figure 1-Figure 5 , a polyvinylidene fluoride device with an embedded pipe, the device comprises: a polyvinylidene fluoride body, an embedded pipe and a central mechanism, the polyvinylidene fluoride body is a prism, a central mechanism is arranged at the center of the prism, the central mechanism comprises a central pipe 05, the central pipe 05 is arranged on the midline of the prism, and the central pipe 05 extends from the center of the prism to the bottom surface 04 of the prism, and penetrates the bottom surface 04 of the prism, the surrounding of the central mechanism is connected with an embedded pipe 02, the embedded pipe 02 extends from the edge of the central mechanism to the edge surface 03 of the prism, and the embedded pipe penetrates the edge surface 03 of the prism, the inner wall of the embedded pipe and the inner wall of the central mechanism are both rough surfaces, the outer surface of the polyvinylidene fluoride body is a smooth surface, including its top surface 01 which is also a smooth surface, and the embedded pipe 02 and the central mechanism are through-connected;
[0050] Among them, the central mechanism also includes a hollow cavity, a central pipe 05 is connected to the bottom center of the hollow cavity, and embedded pipes 02 are connected to the four sides of the hollow cavity; the polyvinylidene fluoride body is a regular prism, and the embedded pipes 02 are all arranged on the central plane of the polyvinylidene fluoride body, the number of embedded pipes 02 is equal to the number of edge faces 03 of the prism, the center point of the edge face 03 of the prism is on the center line of the embedded pipe 02, the inner wall of the embedded pipe 02 is a rough surface of a micro-nano structure, and the inner wall of the central mechanism is a rough surface of a micro-nano structure. The embedded pipe 02 and the central mechanism both use the polyvinylidene fluoride body as the inner wall, the polyvinylidene fluoride body, the embedded pipe 02 and the central mechanism are integrally formed, and the diameter of the embedded pipe 02 is not greater than 1 / 3 of the thickness of the polyvinylidene fluoride body.
[0051] See also Figure 6 As shown, a method for preparing a polyvinylidene fluoride device with an embedded pipeline, the specific steps are as follows:
[0052] Step 1: Making round blank 11
[0053] A round ingot made of polyvinylidene fluoride (PVDF) is selected, placed on a cutting machine for cutting, and a cutting saw is selected to cut the round ingot into a round blank of the required thickness;
[0054] Step 2: Making prismatic embryos 12
[0055] Select the round blank of step 1, put it on the stage of the cutting machine, select a straight cutting saw to cut the equilateral prism, cut the equilateral prism, and then mill the surface of the equilateral prism, put it on the milling machine for milling to obtain the flatness of each surface, mill the chamfer, and then polish it. Use mechanical polishing technology and laser scanning technology to first mechanically polish the flat surface with oilstone to obtain an equilateral prism with the required smoothness, and then perform laser heating scanning on the surface to repair the micro-nano traces of surface damage, and further melt and solidify the surface to obtain a flat, smooth and undamaged surface, which is called a polyvinylidene fluoride body;
[0056] Step 3: Making the first embedded guide hole 13
[0057] Select the polyvinylidene fluoride body of step 2, place its first edge face on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, the buffer pad and the fixture are used to stabilize and protect the polyvinylidene fluoride body, fix the polyvinylidene fluoride body, start the drill bit at the center of the first edge face relative to the edge face, and drill the first embedded guide hole along the straight line between the center of the edge face and the center of the polyvinylidene fluoride body, and drill to the center of the polyvinylidene fluoride body;
[0058] Step 4: Make the embedded guide holes 14 on the remaining edges
[0059] Select the polyvinylidene fluoride body of step 3, and process the embedded guide holes at the centers of the remaining edge faces according to the processing method of step 3 to form embedded guide holes that gather at the center of the polyvinylidene fluoride body and diverge from the edge faces, and drill the embedded guide holes of the polyvinylidene fluoride body;
[0060] Step 5: Make the central guide hole 15 on the bottom surface of the polyvinylidene fluoride body
[0061] Select the polyvinylidene fluoride body of step 4, place its top surface on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, the buffer pad and the fixture are used to stabilize and protect the polyvinylidene fluoride body, fix the polyvinylidene fluoride body, start the drill bit at the center of the top surface relative to the bottom surface, and drill along the center line of the prism to the convergence of the embedded guide holes at the center of the polyvinylidene fluoride body to obtain the interconnection between the central guide hole and the embedded guide hole. At this time, the inner wall of each processed guide hole and the central hollow cavity has many burrs, which will greatly affect the circulation of water and the long-term use of the cooling device;
[0062] Step 6: Making the first embedded pipe 16
[0063] Select the polyvinylidene fluoride body of step 5, place its first edge face on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, the buffer pad and the fixture are used to stabilize and protect the polyvinylidene fluoride body, fix the polyvinylidene fluoride body, and pour paraffin liquid at the first embedded guide hole to fill the first embedded guide hole. Since the temperature of the paraffin liquid is much lower than the melting point of the polyvinylidene fluoride, it will not cause serious damage to the polyvinylidene fluoride on the wall of the first embedded guide hole. Since the first embedded guide hole is a thin and long guide hole, and the thermal conductivity of the polyvinylidene fluoride body is weak, the cooling of the liquid paraffin is very slow. Therefore, some cooling gases (dry ice, nitrogen, etc.) are used for rapid cooling and solidification (using induction The cooling gas can also solidify the burrs caused by the processing of the first guide hole. Liquid paraffin can quickly solidify the burrs. Since paraffin is added as an auxiliary agent during the manufacture of the polyvinylidene fluoride material, the processed polyvinylidene fluoride material will contain a small amount of paraffin. Then, the filled paraffin can be used. According to the principle of attraction of substances, some paraffin can enter the polyvinylidene fluoride body. Then, a drill bit with a diameter 0.15-0.2mm larger than that of the drill bit for processing the guide hole is used for drilling. The drill is drilled to the confluence of the embedded guide holes at the center of the polyvinylidene fluoride body to complete the preparation of the first embedded pipeline. During the drilling process, paraffin will also play a lubricating and grinding role. When the drill bit is drilling, the inner surface of the micro-nano structure will be formed.
[0064] Step 7: Make the embedded pipes 17 on the remaining edges
[0065] Select the polyvinylidene fluoride body of step 6, and process the embedded pipes at the center of the remaining facets according to the processing method of step 6 to form embedded pipes gathered at the center of the polyvinylidene fluoride body and diverging from the facets, and drill the embedded pipes of the polyvinylidene fluoride body;
[0066] Step 8: Make the central embedded pipe 18 on the bottom surface of the polyvinylidene fluoride body
[0067] Select the polyvinylidene fluoride body of step 7, place its top surface on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, the buffer pad and the fixture are used to stabilize and protect the polyvinylidene fluoride body, fix the polyvinylidene fluoride body, and pour paraffin liquid into the central guide hole, fill the central guide hole with paraffin liquid, and use some cooling gas (dry ice, nitrogen, etc.) to quickly cool and solidify (using the blowing method at the guide hole). Since paraffin is added as an auxiliary agent during the manufacture of the polyvinylidene fluoride material, the processed polyvinylidene fluoride material will contain a small amount of paraffin component, and then use the filled paraffin. The principle of attraction of substances allows some paraffin to enter the polyvinylidene fluoride body, and then use a drill bit with a diameter 0.15-0.2mm larger than the drill bit for processing the guide hole to drill to the embedded pipe confluence at the center of the polyvinylidene fluoride body to complete the preparation of the central embedded pipe;
[0068] Step 9: Detection 19
[0069] After the inner side of the embedded pipe is cut open, no obvious burrs are observed under a 20x magnifying glass, and after the hollow cavity is cut open, no obvious burrs are observed under a 20x magnifying glass, achieving an effective use effect; Figure 7 As shown, under the contact angle tester, the surface contact angle of the device is measured to be about 65° ( Figure 7 A), the surface contact angle of the inner wall of the embedded pipe was measured to be around 140° ( Figure 7 B).
[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a polyvinylidene fluoride device with an embedded pipe, characterized in that: The steps are as follows: Step 1: Making the round billet Select a round ingot made of polyvinylidene fluoride (PVDF), put it into a cutting machine for cutting, and select a cutting saw to cut the round ingot into a round blank of the required thickness; Step 2: Making prismatic embryos Select the round blank of step 1, put it on the stage of the cutting machine, select a straight cutting saw to cut the equilateral prism, cut the equilateral prism, and then mill the surface of the equilateral prism, put it on the milling machine for milling, and then mill the chamfer, and then polish it, use mechanical polishing technology and laser scanning technology, first mechanically polish the flat surface with oilstone, and then perform laser heating scanning on the surface to prepare the polyvinylidene fluoride body; Step 3: Make the first embedded guide hole Select the polyvinylidene fluoride body of step 2, place its first edge face on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, fix the polyvinylidene fluoride body, start the drill bit at the center of the first edge face relative to the edge face, and drill the first embedded guide hole along the straight line between the center of the edge face and the center of the polyvinylidene fluoride body, and drill to the center of the polyvinylidene fluoride body; Step 4: Make the embedded guide holes on the remaining edges Select the polyvinylidene fluoride body of step 3, and process the embedded guide holes at the centers of the remaining edge faces according to the processing method of step 3 to form embedded guide holes that gather at the center of the polyvinylidene fluoride body and diverge from the edge faces, and drill the embedded guide holes of the polyvinylidene fluoride body; Step 5: Make the center guide hole on the bottom surface of the PVDF body Select the polyvinylidene fluoride body of step 4, place its top surface on the stage of the drilling machine, and place a fixture with a cushion on the stage, fix the polyvinylidene fluoride body, start the drill bit at the center of the top surface relative to the bottom surface, and drill along the center line of the prism to the convergence of the embedded guide holes at the center of the polyvinylidene fluoride body to obtain the interconnection between the central guide hole and the embedded guide hole; Step 6: Make the first embedded pipe Select the polyvinylidene fluoride body of step 5, place its first edge face on the stage of the drilling machine, and place a fixture with a buffer pad on the stage, fix the polyvinylidene fluoride body, and pour paraffin liquid at the first embedded guide hole, fill the first embedded guide hole with paraffin liquid, use some cooling gas to quickly cool and solidify, and then use a drill bit with a diameter 0.15-0.2mm larger than the drill bit for machining the guide hole to drill to the confluence of the embedded guide holes at the center of the polyvinylidene fluoride body, and complete the preparation of the first embedded pipeline; Step 7: Make the embedded pipes on the remaining edges Select the polyvinylidene fluoride body of step 6, and process the embedded pipes at the center of the remaining facets according to the processing method of step 6 to form embedded pipes gathered at the center of the polyvinylidene fluoride body and diverging from the facets, and drill the embedded pipes of the polyvinylidene fluoride body; Step 8: Make the center embedded pipe on the bottom surface of the PVDF body Select the polyvinylidene fluoride body of step 7, place its top surface on the stage of the drilling machine, and place a tooling fixture with a cushion on the stage, fix the polyvinylidene fluoride body, and pour paraffin liquid into the center guide hole. Fill the center guide hole with paraffin liquid, use some cooling gas to quickly cool and solidify it, and then use a drill bit with a diameter 0.15-0.2mm larger than the drill bit for processing the guide hole to drill to the embedded pipe confluence at the center of the polyvinylidene fluoride body to complete the preparation of the center embedded pipe.
Citation Information
Patent Citations
Water cooling heat radiator
CN105023895A
Flow-dividing annular micro-channel radiator
CN107658281A
Strong and tough structural wood materials, and methods for fabricating and use thereof
CN110914029A
Method for making a micro milling tool comprising integrated cooling channels
EP3741500A1
Armature for fire fighting and / or cooling of burning objects
WO2020253909A1