A method for preparing thermal transfer carbon ribbon suitable for glass substrate
By using thermal transfer carbon tape process on glass substrates and combining multi-layer coating technology, the damage rate and pollution problems of high-temperature printing in existing glass decorative technologies are solved, and efficient and personalized pattern printing is achieved, which improves the product scratch resistance and adhesion.
Patent Information
- Application Number
- CN202211414237.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-11
AI Technical Summary
In the existing glass decoration technology, the high-temperature printing process has a high breakage rate and the risk of heavy metal poisoning. The screen printing process is low in efficiency and monotonous in graphics and text, which cannot meet personalized needs, and there are problems of energy conservation, emission reduction and pollution.
By adopting a thermal transfer carbon tape preparation method suitable for glass substrates, by printing the pattern onto the carbon tape and transferring it to the glass substrate, combining the protective layer, dye receiving layer, release layer and follow-up layer, Achieve efficient and personalized pattern printing.
It improves operation simplicity and efficiency, reduces energy consumption and pollution, meets personalized needs, and improves scratch resistance and adhesion of the pattern.
Smart Images

Figure CN115556493B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of soft label printing, and in particular relates to a method for preparing a thermal transfer carbon ribbon suitable for a glass substrate. Background Art
[0002] The glass printing process is a form of glass decoration technology that prints patterns onto glass through high temperature. Currently, the commonly used processes are high-temperature printing or screen printing. Among them, the products produced by high-temperature printing have excellent stability, strong surface scratch resistance, and good water resistance, but the process often involves high temperatures, a high breakage rate, and a risk of heavy metal poisoning; the products produced by screen printing have good water resistance and a high yield, but there are also defects such as low production efficiency and monotonous printed images.
[0003] Therefore, a preparation method of a thermal transfer carbon ribbon suitable for a glass substrate and a preparation method thereof are proposed to solve the deficiencies in the prior art. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a thermal transfer carbon ribbon suitable for a glass substrate. The printed thermal transfer carbon ribbon is hot-stamped onto a glass substrate. The operation is simple and efficient. While restoring the color of the pattern itself, different patterns can be printed according to the personalized needs of different users. Compared with traditional high-temperature printing, this process has the advantages of energy saving, emission reduction and pollution reduction.
[0005] The technical solution of the present invention to solve the above technical problems is as follows: The preparation method of the thermal transfer carbon ribbon suitable for glass substrate includes S1: printing the required pattern on carbon ribbon A in a mirror image to obtain carbon ribbon A with a pattern; S2: transferring the carbon ribbon B obtained in S2 to the carbon ribbon A with a pattern to obtain a thermal transfer carbon ribbon; S3: thermally mounting and transferring the thermal transfer carbon ribbon obtained in S2 to a glass substrate to obtain a finished product.
[0006] Beneficial effects: The required pattern is first printed on carbon ribbon A, and then carbon ribbon B is transferred to carbon ribbon A with the pattern. The obtained thermal transfer carbon ribbon is heat-mounted and transferred to the glass substrate. The printed thermal transfer carbon ribbon is hot-stamped on the glass substrate. The operation is simple and efficient. While restoring the color of the pattern itself, different patterns can be printed according to the personalized needs of different users. Compared with traditional high-temperature printing, this process has the advantages of energy saving, emission reduction and pollution reduction.
[0007] Based on the above technical solution, the present invention can also be improved as follows.
[0008] Further, in step S1, the carbon ribbon A includes a first substrate, a protective layer and a dye receiving layer which are sequentially arranged from bottom to top.
[0009] Beneficial effect: used to transfer the desired pattern onto carbon ribbon A.
[0010] Furthermore, the protective layer is made by the following steps: dissolving at least one of acrylic resin, polyurethane resin, epoxy resin and polyester resin with 2-butanone and toluene to prepare a protective layer coating, applying the protective layer coating to the base of the protective layer and drying it to form a protective layer.
[0011] Beneficial effects: Protect the integrity of the pattern layer and improve its scratch resistance, weather resistance and solvent resistance.
[0012] Furthermore, the dye receiving layer is made by the following steps: dissolving at least one of ethylene-vinyl acetate copolymer, polyester resin, acrylic resin, polyolefin resin, polyurethane resin, and vinyl chloride vinyl acetate with 2-butanone and toluene to prepare a dye receiving coating, applying the dye receiving coating to the base of the dye receiving layer and drying it to form the dye receiving layer.
[0013] Beneficial effect: It is easy to combine with patterns to form a pattern layer.
[0014] Further, in step S2, the carbon ribbon B includes a second substrate, a release layer and a bonding layer which are sequentially arranged from bottom to top.
[0015] Beneficial effect: It is easy to combine with the carbon ribbon A with a pattern to obtain a thermal transfer carbon ribbon.
[0016] Furthermore, the release layer is made by the following steps: dissolving at least one of polyester resin, acrylic resin, EVA resin, ethylene-vinyl acetate copolymer, and polyvinyl alcohol with 2-butanone and toluene to prepare a release liquid coating, applying the release liquid coating to the base of the release layer and drying it to form a release layer.
[0017] Beneficial effect: Helps the adhesive layer to be better separated from the substrate.
[0018] Furthermore, the adhesive layer is made by the following steps: dissolving at least one of polyester resin, acrylic resin, polyurethane resin, ethylene-vinyl acetate copolymer, epoxy resin, silane coupling agent, and epoxy phosphate coupling agent with 2-butanone and toluene to prepare an adhesive liquid coating, applying the adhesive liquid coating to the substrate of the adhesive layer and drying it to form the adhesive layer.
[0019] Beneficial effect: Increase the adhesion between the pattern and the glass substrate.
[0020] Furthermore, the first substrate and the second substrate are any one of polyethylene terephthalate film, polyacrylonitrile-butadiene-styrene film, polyethylene naphthalate film, polystyrene film, polypropylene film, polyethylene film, nylon film, and polyimide film.
[0021] Beneficial effect: Using the above film as a substrate can better ensure that each layer can be effectively coated on the surface of the substrate.
[0022] Furthermore, the thickness of the first substrate and the second substrate are both 1-30 μm.
[0023] Beneficial effect: Ensure successful pattern reception and thermal transfer.
[0024] Furthermore, the thickness of the protective layer is 5-20 μm, the thickness of the dye receiving layer is 5-20 μm, the thickness of the release layer is 0.1-10 μm, and the thickness of the adhesive layer is 0.1-10 μm.
[0025] Beneficial effect: The thickness of the thermal transfer ribbon can be guaranteed within this thickness range, and at the same time, the adhesion and wear resistance to the substrate are good. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the layer structure of the carbon ribbon of the present invention;
[0027] Figure 2 Schematic diagram of the layer structure of the carbon ribbon A of the present invention;
[0028] Figure 3 Schematic diagram of the layer structure of the carbon ribbon B of the present invention. DETAILED DESCRIPTION
[0029] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0030] Embodiment 1:
[0031] This embodiment provides a method for preparing a thermal transfer carbon ribbon suitable for a glass substrate, comprising:
[0032] The following steps;
[0033] S1: Print the desired pattern on the carbon ribbon A in a mirror image to obtain the carbon ribbon A with the pattern;
[0034] S2: Transferring the carbon ribbon B onto the carbon ribbon A with the pattern to obtain a thermal transfer carbon ribbon;
[0035] S3: thermally transfer the thermal transfer carbon ribbon of S2 onto the glass substrate 4 to obtain a finished product.
[0036] Wherein, the substrate is polyethylene terephthalate with a thickness of 4.3 μm;
[0037] Specifically, in step S1, the carbon ribbon A is manufactured by:
[0038] The protective layer 2 is made by the following steps:
[0039] Weigh 10 parts of acrylic resin by weight, then dissolve it with 2-butanone and toluene, add a certain amount of dispersant and mix well to prepare a protective layer coating with a solid content of 10%; then use a 200-line ceramic anilox roller and a gravure coater to coat the protective layer coating on the lower side of the substrate and dry it to a thickness of 0.3 μm, wherein the 2-butanone in the mixed solvent is 50% and the toluene is 50%.
[0040] The dye receiving layer 3 is made by the following steps:
[0041] Weigh 9 parts by weight of ethylene-vinyl acetate copolymer and 1 part of polyurethane, then dissolve them with 2-butanone and toluene to prepare a dye receiving layer coating with a solid content of 20%; then use a 120-line ceramic anilox roller and a gravure coater to coat the dye receiving layer coating on a substrate containing a protective layer 2, cover the protective layer and dry it, with a thickness of 1-2 μm, wherein the 2-butanone in the mixed solvent is 50% and the toluene is 50%.
[0042] In step S2, the carbon ribbon B is made by the following steps:.
[0043] The release layer 6 is made by the following steps:
[0044] Weigh 10 parts by weight of epoxy resin and 1 part of reactive silicone oil, then dissolve them with 2-butanone and toluene to prepare a release layer coating with a solid content of 10%; then use a 200-line ceramic anilox roller and a gravure coater to coat the release layer coating on the lower side of the substrate and dry it to a thickness of 0.5 μm, wherein the 2-butanone in the mixed solvent is 50% and toluene is 50%.
[0045] The adhesive layer 7 is made by the following steps:
[0046] Weigh 5 parts of polyester, 5 parts of epoxy resin, and 1 part of silane coupling agent, then dissolve them with 2-butanone and toluene to prepare a bonding layer coating with a solid content of 20%; then use a 120-line ceramic anilox roller and a gravure coater to coat the bonding layer coating on a substrate containing a release layer 6, cover the release layer, and dry it to a thickness of 1 μm, wherein the 2-butanone in the mixed solvent is 50% and the toluene is 50%.
[0047] Embodiment 2:
[0048] The difference between this embodiment and embodiment 1 is that the mass ratio of ethylene-vinyl acetate copolymer to polyurethane in the dye receiving layer 3 is 8:2 or 7:3.
[0049] Embodiment 3:
[0050] The difference between this embodiment and embodiment 1 is that 10 parts of epoxy resin in the release layer 6 are replaced by 10 parts of acrylic resin.
[0051] Embodiment 4:
[0052] The difference between this embodiment and embodiment 1 is that the mass ratio of polyester to epoxy resin in the adhesive layer 7 is 9:1 or 8:2 or 7:3 or 6:4, and the amount of silane coupling agent added is 3 parts or 5 parts.
[0053] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0054] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a thermal transfer ribbon suitable for a glass substrate, characterized in that: The steps include: S1: Print the desired pattern on the carbon ribbon A in a mirror image to obtain the carbon ribbon A with the pattern; S2: Transferring the carbon ribbon B onto the carbon ribbon A with the pattern obtained in S1 to obtain a thermal transfer carbon ribbon; S3: thermally transfer the thermal transfer carbon ribbon obtained in S2 onto a glass substrate (4) to obtain a finished product; In step S1, the carbon ribbon A comprises a first substrate (1), a protective layer (2) and a dye receiving layer (3) which are arranged in sequence from bottom to top; In step S2, the carbon ribbon B comprises a second substrate (5), a release layer (6) and a bonding layer (7) which are arranged in sequence from bottom to top.
2. The method for preparing a thermal transfer ribbon suitable for a glass substrate according to claim 1, characterized in that: The protective layer (2) is made by the following steps: At least one of acrylic resin, polyurethane resin, epoxy resin and polyester resin is dissolved in 2-butanone and toluene to prepare a protective layer coating, and the protective layer coating is applied to the protective layer substrate and dried to form a protective layer (2).
3. The method for preparing a thermal transfer ribbon suitable for a glass substrate according to claim 1, characterized in that: The dye receiving layer (3) is made by the following steps: At least one of ethylene-vinyl acetate copolymer, polyester resin, acrylic resin, polyolefin resin, polyurethane resin, and vinyl chloride vinyl acetate is dissolved in 2-butanone and toluene to prepare a dye receiving coating, and the dye receiving coating is applied to the substrate of the dye receiving layer (3) and dried to form the dye receiving layer (3).
4. The method for preparing a thermal transfer ribbon suitable for glass substrate according to claim 1, characterized in that: The release layer (6) is made by the following steps: At least one of polyester resin, acrylic resin, ethylene-vinyl acetate copolymer and polyvinyl alcohol is dissolved in 2-butanone and toluene to prepare a release liquid coating, and the release liquid coating is applied to the substrate of the release layer (6) and dried to form the release layer (6).
5. The method for preparing a thermal transfer ribbon suitable for glass substrate according to claim 4, characterized in that: The bonding layer (7) is made by the following steps: At least one of polyester resin, acrylic resin, polyurethane resin, ethylene-vinyl acetate copolymer, epoxy resin, silane coupling agent and epoxy phosphate coupling agent is dissolved in 2-butanone and toluene to prepare an adhesive liquid coating, and the adhesive liquid coating is applied to the substrate of the adhesive layer (7) and dried to form the adhesive layer (7).
6. The method for preparing a thermal transfer ribbon suitable for glass substrate according to claim 4, characterized in that: The first substrate (1) and the second substrate (5) are any one of polyethylene terephthalate film, polyacrylonitrile-butadiene-styrene film, polyethylene naphthalate film, polystyrene film, polypropylene film, polyethylene film, nylon film, and polyimide film.
7. The method for preparing a thermal transfer ribbon suitable for a glass substrate according to claim 6, characterized in that: The thickness of the first substrate (1) and the second substrate (5) are both 1-30 μm.
8. The method for preparing a thermal transfer ribbon suitable for glass substrate according to claim 6, characterized in that: The thickness of the protective layer is 5-20 μm, the thickness of the dye receiving layer is 5-20 μm, the thickness of the release layer is 0.1-10 μm, and the thickness of the adhesive layer is 0.1-10 μm.