A two-component composite elastic fiber capable of being dyed at low temperature and normal pressure and a preparation method thereof
By selecting low-temperature and normal-pressure dyeable polyester with good compatibility and heat shrinkage difference, and combining the spinning-stretching-heat-setting process, a side-by-side composite fiber with a permanent spiral three-dimensional curl structure is formed, which solves the current problem. There is a problem in the technology that fibers cannot be effectively dyed in low temperature environments, and the excellent fastness and elastic properties of dark dyes have been improved.
Patent Information
- Application Number
- CN202110318541.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-25
AI Technical Summary
Existing side-by-side composite fibers cannot be dyed effectively in low-temperature environments, especially the PET component that cannot be dyed below 130°C, resulting in defects in elastic fabrics blended or interwoven with fibers such as cotton, wool, and silk that are not resistant to high temperatures. , and high-temperature dyeing will damage the performance of other components.
Two low-temperature and normal-pressure dyeable polyesters with good compatibility and different thermal shrinkage rates are selected as components of the side-by-side composite fiber. A "dumbbell-shaped" cross-section is formed through a spinning-stretching-heat-setting process. Disperse dyes or Cationic dyes are dyed at low temperatures to ensure that the fiber has a permanent spiral three-dimensional curl structure and excellent dyeing fastness under low temperature conditions.
It realizes the dyeing of dark dyes on side-by-side composite fibers under low temperature conditions, meets the needs of blending or interweaving with natural fibers, expands the application fields, and improves the elastic elongation and recovery rate of the fibers, avoiding the harmful effects of high-temperature dyeing. Damage to fabric properties.
Abstract
Description
Technical Field
[0001] The present invention is an elastic polyester fiber with a spiral three-dimensional curling structure and a preparation method thereof. The elastic fiber is a parallel composite fiber composed of two low-temperature and normal pressure dyeable polyesters with good compatibility and different heat shrinkage rates. After the fiber is subjected to a wet heat treatment such as low-temperature and normal pressure dyeing, a permanent spiral three-dimensional curling morphology structure can be obtained, thereby giving the fiber good elastic elongation and elastic recovery rate. Different from similar parallel composite fibers in the past, its two components can be dyed with disperse dyes or cationic dyes at low temperature and normal pressure to a full color spectrum including black, dark brown, navy blue and other dark colors, and have excellent color fastness; therefore, the elastic fiber is very suitable for blending or interweaving elastic fabrics with natural fibers such as cotton, wool, hemp, silk and viscose fibers, nylon chemical fibers and other fibers that are not resistant to high temperature dyeing. The dyeing requirements must be met at low temperature and normal pressure to protect their functions; it is also more suitable for low temperature and normal pressure dyeing with new disperse dyes, iterative polyester-D, polyester (ECDP) fibers dyeable with low temperature and normal pressure cationic dyes, and new low temperature and normal pressure iterative polyester-C (NECDP) blended or interwoven elastic fabrics, thereby expanding and expanding the application field of parallel composite elastic fibers. Low temperature and normal pressure dyeing also has the economic and social benefits of energy saving and emission reduction. Background Art
[0002] There are many research works on polymer elastic fibers, but only a limited number of them can be industrialized and applied. The most famous one is "Lycra" of Du Pont Company in the United States; and T-400 is another new elastic fiber product developed by Du Pont. T-400 is a PET / PTT two-component parallel composite fiber with a dumbbell-shaped cross section. Because the two components have different thermal shrinkage properties and an asymmetric cross section, when the fiber is heat-treated, it will produce permanent spiral curling. This three-dimensional spiral curling determined by its own properties makes the fiber have good elastic elongation and elastic recovery. Compared with "Lycra", this spiral curled elastic fiber has many characteristics. Its elastic elongation (about 50%~150%) and elastic recovery rate (about 80% when elongated by 25%) are obviously not as good as Lycra, but it is enough to meet the needs of elastic woven or knitted fabrics. However, compared with Lycra, it has many advantages. Its processing technology is simple, the production process is short, it is pollution-free and environmentally friendly; it has high strength, which is conducive to textile processing; it has low modulus, so it does not put pressure on the human body when wearing clothes; it has good heat resistance and can be dyed in the same bath as ordinary polyester, and it will not lose elasticity due to dyeing; it has good light resistance; it is resistant to chlorine bleaching; and it has low raw material cost and is cheap. Therefore, it can complement Lycra in terms of application, and its price advantage has strong market competitiveness.
[0003] In recent years, the production and demand for parallel composite fibers have been very active. In addition to the PET / PTT combination with the same components as T-400, more research and development work is being done on the combination of raw materials for parallel composite fibers, and most of the research and development is mainly to reduce production costs. For example, the patents of "A high-low viscosity PET parallel composite self-curling fiber and its preparation method" with publication number CN111101237A, "A parallel composite PBT polyester fiber and its preparation method" with publication number CN106337212A, and "A PBT / PET two-component elastic composite fiber production process" with publication number 107964690A, etc. There are also patent applications disclosing "A parallel composite elastic fiber and its preparation method", which has a peanut-shaped parallel structure in cross section, and is a fiber formed by extruding and compounding 2,6-naphthalene dicarboxylic acid copolymer modified PET and 2,6-naphthalene dicarboxylic acid copolymer modified PTT at a mass ratio of 45-55:55-45. No matter which of the above two-component combinations is separated from the PET component with a higher glass transition temperature, there is a major drawback, that is, the PET component can only be dyed at a high temperature of 125°C to 130°C. If natural fibers such as cotton, wool, hemp, silk, and chemical fibers such as viscose fibers and nylon that can only be dyed at an environment below 100°C are blended or interwoven with the elastic fiber to form an elastic fabric, the low-temperature dyeing process will reveal its shortcomings, that is, the PET component cannot be dyed and turns white. Although dyeing at a high temperature of 125°C to 130°C can avoid the whitening of PET fibers, it will inevitably damage the performance of another component in the above-mentioned blended or interwoven elastic fabric, and will also reduce the excellent elasticity of the elastic fiber itself. In recent years, the new disperse dye normal pressure deep-dyeable iterative polyester-D and the new low-temperature normal pressure cationic dye deep-dyeable iterative polyester-C (NECDP) developed by the patent applicant have created good conditions for energy saving, emission reduction, and low-temperature deep-dyeing. The low-temperature deep-dyeable parallel composite elastic fiber of this patent can be used to weave elastic fabrics. The significance of the present invention lies in that by selecting a suitable parallel composite two-component combination, good elasticity can be obtained through the two-component parallel composite spinning, and a full color spectrum including dark colors such as black, dark brown, navy blue, etc. can be dyed with disperse dyes or cationic dyes at low temperature and normal pressure, and the color fastness is excellent, so that the requirements for dyeing elastic fabrics blended or interwoven with natural fibers including cotton, wool, hemp, silk, and viscose fibers, nylon-type chemical fibers, etc. that are not resistant to high temperature dyeing can be met. The present invention is also suitable for low temperature and normal pressure one-bath dyeing of blended or interwoven elastic fabrics with new disperse dye normal pressure deep-dyeable iterative polyester-D, low temperature and normal pressure cationic dye dyeable polyester (ECDP), and new low temperature and normal pressure cationic dye deep-dyeable polyester (NECDP), thereby expanding and expanding the application field of the parallel composite elastic fiber. Summary of the invention
[0004] In order to prepare a two-component parallel composite fiber with a permanent good elastic function of a spiral three-dimensional curled structure, the two selected polymer components have good compatibility, which is a necessary condition for forming a parallel structure; the two components constituting the parallel composite fiber should also have a large difference in thermal shrinkage; the cross-sectional morphology of the parallel composite fiber is "dumbbell-shaped", which is conducive to the formation of the best spiral three-dimensional curled structure; the parallel composite fiber can only obtain the best elastic effect under suitable heat treatment conditions. Among them, if the two components constituting the parallel composite fiber are to have a large difference in thermal shrinkage, it is necessary to select a suitable combination of two-component raw materials and spinning-stretching-heat setting process conditions corresponding to the raw material properties. Previous similar two-component parallel composite fibers, such as Dupont's PET / PTT two-component composite T-400, PET with two different high and low intrinsic viscosities, PET / modified PET and PET / PBT, etc., no matter which two-component combination, have not been separated from PET, so there is a major drawback, that is, the PET component must be dyed at 130°C. This limits its scope of application. For example, when they are used in blended or interwoven elastic fabrics with natural fibers such as cotton, wool, hemp, silk, and viscose fibers, nylon chemical fibers that are not resistant to high temperature dyeing, or blended or interwoven elastic fabrics with new disperse dye normal pressure deep dyeable iterative polyester-D and low temperature normal pressure cationic dye dyeable polyester (ECDP) fiber, and new low temperature normal pressure cationic dye deep dyeable iterative polyester-C, when the above-mentioned two-component composite elastic fibers are dyed at low temperature and normal pressure, the PET component therein cannot be dyed and turns white, which brings defects to the fabric quality.
[0005] In order to solve the above problems, it is necessary to re-synthesize or select suitable raw materials for two-component parallel composite spinning, which needs to meet three conditions: (1) The two components must have good compatibility; (2) During the spinning-stretching-setting process, one of the two components must have a highly oriented and crystalline supramolecular structure; while the other component should be in a potential high-shrinkage supramolecular structure that is only highly oriented but not yet crystallized or low in crystallization. Among the two components, the orientation degree f of the high-oriented, low-crystalline structure component is not less than 0.75, and the crystallinity Xc is not higher than 40%; the orientation degree f of the low-oriented, high-crystalline structure component is not greater than 0.50, and the crystallinity Xc is not less than 46%. In this way, after the fiber is formed, when it is subjected to heat treatment again (such as wet heat dyeing process), it will form a permanent spiral three-dimensional curled structure state due to the difference in thermal shrinkage between the two, giving it elasticity; (3) The selected two components must be dyeable at low temperature and normal pressure using disperse dyes or cationic dyes.
[0006] The raw material combinations selected in the present invention include copolyesters HSPET with poor structural regularity, which are prepared by using terephthalic acid (PTA) and ethylene glycol (EG) as basic raw materials, adding appropriate amounts of isophthalic acid (IPA) with an meta structure and / or neopentyl glycol (DTG) containing a side group structure, and / or cyclohexanedimethanol (CHDM), etc., and the crystallization temperature of its differential thermal analysis (DSC) curve exceeds 160°C, and the crystallization peak is flat and difficult to crystallize; PBT with a high relative molecular weight; PTT with a high relative molecular weight; cationic dye normal pressure dyeable polyesters (ECDP) with different relative molecular weights; new disperse dye normal pressure deep dyeable polyesters (NEDDP) with different relative molecular weights and new cationic dye normal pressure deep dyeable polyesters (NECDP) with different relative molecular weights.
[0007] On the basis of selecting the raw material compatibility, a complete set of spinning-stretching-heat setting process conditions must be set according to the relative molecular mass and thermal properties of different raw materials, so as to give the two component fibers of the parallel composite fiber a supramolecular structure with high orientation and low crystallinity and high orientation and high crystallinity respectively.
[0008] The high shrinkage fiber copolyester (HSPET) and polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), new disperse dye normal pressure deep dye polyester (NEDDP), cationic dye normal pressure dye polyester (ECDP), new cationic dye normal pressure deep dye polyester (NECDP) and the above-mentioned polyesters with different high and low intrinsic viscosities are used as raw materials to form a parallel composite fiber. The volume composition ratio of the two components can be selected in the range of 35 / 65~65 / 35, preferably 50 / 50. The above two polyester components are selected and combined according to the predetermined ratio using the parallel melt composite spinning technology, and the parallel composite fiber is obtained through spinning-stretching-heat setting. The fiber is heat-treated again to obtain a permanent spiral three-dimensional curling structure elastic fiber, which increases the curling number per unit fiber length and reduces the curling radius, showing better elastic elongation and elastic recovery rate. Depending on the selected raw material combination, the melt spinning temperature can be controlled in the range of 265℃~295℃, the spinning speed can be controlled in the range of 1,000~3,000 m / min, the stretching temperature in the range of 60℃~100℃, the stretching multiple in the range of 3.8~1.8 times, and the setting temperature in the range of 90℃~170℃. By controlling the reasonable fiber forming processing technology, different orientations and crystal structures can be given to the two components constituting the parallel composite fiber.
[0009] The fiber that has been spun, stretched and fixed is heat treated again in a relaxed state to obtain better elastic elongation and elastic recovery properties. The heat treatment can be a wet heat treatment in hot water or a dry heat treatment. The hot water treatment temperature is preferably 85℃~100℃, which can be combined with the dyeing and finishing process of the fabric. However, the best elastic elongation and elastic recovery rate cannot be obtained if the heat treatment temperature is too high or too low. The elastic elongation of the fiber after heat treatment can reach 80%~120%, and the elastic recovery rate varies depending on the composition of the raw materials, ranging from 82%~94%; the fiber has good resistance to multiple tensile deformation elastic recovery fatigue performance. DETAILED DESCRIPTION
[0010] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0011] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0012] Embodiment 1:
[0013] The sliced raw materials used are HSPET with a characteristic viscosity of 0.675 dl / g and a melting point of 248°C, and PTT with a characteristic viscosity of 0.91 dl / g and a melting point of 225°C. The two slices are pre-crystallized and dried first, and then the parallel composite fibers are spun using a twin-screw composite spinning machine. The diameter of the two screws is 30 mm, the aspect ratio is 25:1, the main and auxiliary double-box structure, and the spinning spinneret is a 24-hole spinning spinneret made by Kazunozu with a hole diameter of 0.25 mm. The volume ratio of the two components is selected to be 50 / 50, the spinning box temperature is 276°C, and the spinning speed is 1,000 m / min. The winding yarn is stretched and set on a flat drawing machine, with a stretching temperature of 90°C, a stretching multiple of 3.8 times, and a setting temperature of 150°C. The finished fiber has a linear density of 150dtex / 48f, a breaking strength of 2.56cN / dtex, an elongation at break of 12%, and a "dumbbell-shaped" cross-sectional structure of the parallel composite fiber. After the fiber was immersed in 80℃ hot water for 30min, the elastic elongation was 92%, the elastic recovery was 88%, the number of crimps was 17 / 10cm, and the crimp radius was 0.86mm. The fiber has good resistance to multiple tensile deformation and elastic recovery fatigue performance. The fiber after heat treatment was continuously stretched 120 times (stretching frequency 1 time / min, elongation 25%), and the elastic recovery rate was greater than 85%; the fiber was continuously stretched 60 times (stretching frequency 0.5 times / min, elongation 50%), and the elastic recovery rate was greater than 65%. 5% (owf) disperse blue dye was used for dyeing at 100℃ and 110℃. The color at 110℃ was darker than that at 100℃, indicating that PTT had not yet been deeply dyed at 100℃, and the coloring rate of PTT was improved at 110℃.
[0014] Embodiment 2:
[0015] The sliced raw materials used are HSPET with a characteristic viscosity of 0.625dl / g and a melting point of 248℃, and NEDDP with a characteristic viscosity of 1.062dl / g and a melting point of 245℃. The two slices are pre-crystallized and dried first, and then the parallel composite fibers are spun using a twin-screw composite spinning machine. The screw diameter is 30mm, the aspect ratio is 25:1, the main and auxiliary double box structure, the spinning spinneret is made by Kazunozu, 24 holes, and the spinneret hole diameter is 0.25mm. The volume composition ratio of the two components is selected to be 50 / 50, the spinning temperature is 272℃, and the spinning speed is 1,700m / min. The winding yarn is stretched and set on a flat drawing machine, with a stretching temperature of 90℃, a stretching multiple of 3.0 times, and a setting temperature of 145℃. The finished fiber has a linear density of 150dtex / 48f, a breaking strength of 2.62cN / dtex, an elongation at break of 14%, and a "dumbbell-shaped" cross-sectional structure. After soaking the fiber in 80°C hot water for 30 minutes, the elastic elongation is 94%, the elastic recovery is 86%, the number of curls is 16 / 10cm, and the curl radius is 0.82mm. Dyeing with 5% (owf) disperse blue dye at 100°C yields a satisfactory dark color. The color fastness of the six fibers is above level 4. The dyeing is uniform under an optical microscope, and no whitening is observed.
[0016] Embodiment 3:
[0017] Two NEDDP with characteristic viscosities of 0.503 dl / g and 1.21 dl / g were used as raw materials. The two slices were first pre-crystallized and dried on a continuous dryer, and the moisture content of the slices was 31 ppm. Then, FDY parallel composite fibers were spun using a twin-screw composite spinning machine. The screw diameter was 65 mm, the aspect ratio was 25:1, the main and auxiliary double-box structure, the spinning spinneret was 32 holes, and the spinneret hole diameter was 0.25 mm. The volume ratio of the two components was selected to be 50 / 50, the spinning temperature was 282°C, the temperature of the first hot roller (DR1) was 80°C, and the speed was 1650 m / min; the temperature of the second hot roller (DR2) was 140°C, the speed was 4700 m / min; and the winding speed was 4660 m / min. The finished fiber has a linear density of 50d / 32f, a breaking strength of 3.15cN / dt, an elongation at break of 22.6%, a boiling water shrinkage of 12.0%, an elastic elongation of 73.5%, and a "dumbbell-shaped" cross-sectional structure. After the fiber was relaxed and soaked in hot water at 88°C for 30 minutes, the elastic elongation was 93%, and the elastic recovery was 94%. 5% (owf) disperse red, disperse yellow, disperse blue and disperse black dyes were used for dyeing at 100°C to obtain a satisfactory dark color. The color fastness of the six fibers was above level 4. The dyeing was uniform under an optical microscope, and no whitening was observed.
[0018] Embodiment 4:
[0019] The fibers spun in the above Example 3 and 75d / 72f iterative polyester-D were interlaced with each other using a 48-needle circular mesh knitting machine to form a weft knitted fabric. Then, an overflow dyeing machine was used to dye 5% (owf) disperse blue dye at 98°C for 40 minutes, and then reduction cleaning-water washing-drying was performed to obtain a blue elastic fabric. The color fastness of the six fibers to staining was above level 4. No whitening phenomenon was observed under an optical microscope.
[0020] Embodiment 5:
[0021] Using two ECDPs with characteristic viscosities of 0.481 dl / g and 0.832 dl / g as raw materials, the two slices were pre-crystallized and dried. Then, FDY parallel composite fibers were spun using a twin-screw composite spinning machine. The screw diameter is 30 mm, the aspect ratio is 25:1, the main and auxiliary double-box structures, the spinning spinneret is 24 holes, and the spinneret hole diameter is 0.25 mm. The volume ratio of the two components is selected to be 50 / 50, the spinning temperature is 284°C, and the winding speed is 1350 m / min. The winding yarn is stretched and set on a flat drawing machine, with a stretching temperature of 90°C, a stretching multiple of 3.1 times, and a setting temperature of 146°C. The finished fiber has a linear density of 148dtex / 48f, a breaking strength of 2.13cN / dtex, and a breaking elongation of 15%. The cross-sectional structure of the parallel composite fiber is "dumbbell-shaped". After soaking the fiber in 80℃ hot water for 30min, the elastic elongation is 91%, the elastic recovery is 88%, the number of crimps is 16 / 10cm, and the crimp radius is 0.84mm. The fiber is dyed with 3.0% (owf) cationic brilliant blue dye at 100℃ to obtain a satisfactory dark color. The color fastness of the six fibers is above grade 4. The dyeing is uniform under an optical microscope, and no whitening phenomenon is observed.
[0022] Comparative Example 1:
[0023] The commercially available parallel bicomponent composite fiber with PET / PTT as raw materials has a linear density of 100d / 36f, a breaking strength of 3.23cN / dt, an elongation at break of 32.8%, and a boiling water shrinkage of 9.2%. Another parallel bicomponent composite fiber with the same raw materials has a linear density of 75d / 36f, a breaking strength of 3.0 cN / dt, an elongation at break of 24.6%, a boiling water shrinkage of 10.29%, a compression elongation of 168%, and a compression elastic recovery of 94.48%, with good physical and mechanical properties. After dyeing with 5% (owf) disperse blue dye at 100°C, it was observed under an optical microscope to be blue and white, and the PET part was not dyed. The temperature was continued to be raised to 125°C for dyeing, and no whitening phenomenon was observed under an optical microscope.
[0024] Comparative Example 2:
[0025] The commercially available parallel bicomponent composite fiber with PET / PBT as raw materials has a linear density of 75d / 48f, a breaking strength of 3.23 cN / dt, an elongation at break of 30.2%, and a boiling water shrinkage of 7.4%. Another parallel bicomponent composite fiber with the same raw materials has a linear density of 75d / 36f, a breaking strength of 3.2 cN / dt, an elongation at break of 25.8%, a boiling water shrinkage of 9.15%, a compression elongation of 161%, and a compression elastic recovery of 92.15%, with good physical and mechanical properties. After dyeing with 5% (owf) disperse blue dye at 100°C, it was observed under an optical microscope to show blue and white colors, among which the PET part was not dyed. Continue to increase the temperature to 130°C for dyeing to obtain a blue effect of full dyeing.
[0026] Comparative Example 3:
[0027] The parallel two-component composite fiber with different high and low viscosity PET / PET as raw materials is available on the market. The linear density is 75d / 36f, the breaking strength is 3.62 cN / dt, the breaking elongation is 28.9%, the boiling water shrinkage is 9.5%, and the physical and mechanical properties are good. It is basically not dyed at 100℃ with 4% (owf) disperse blue dye, and only slightly stained. Continue to increase the temperature to 130℃ for dyeing and keep it for 40min to obtain a medium-dark blue effect.
[0028] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A two-component composite elastic fiber that can be dyed at low temperature and normal pressure, characterized in that: The invention comprises two components with good compatibility, wherein the two components are two copolyesters or polyesters capable of being dyed at low temperature. The two components are subjected to spinning-stretching-setting process and heat treatment process to obtain a two-component composite elastic fiber capable of being dyed at low temperature and normal pressure. The volume ratio of the two components is (35:65) to (65:35). The two-component composite elastic fiber comprises a combination of a copolyester for high shrinkage fiber (HSPET) and a new disperse dye normal pressure deep dyeable polyester (NEDDP), a combination of a high intrinsic viscosity new disperse dye normal pressure deep dyeable polyester (NEDDP) and a low intrinsic viscosity new disperse dye normal pressure deep dyeable polyester (NEDDP). The intrinsic viscosity of the copolyester measured by conventional testing methods can be selected within the range of 0.48 to 0.625 dl·g-1 and 1.062 to 1.25 dl·g-1. The method for preparing the two-component composite elastic fiber capable of being dyed at low temperature and normal pressure comprises the following steps: subjecting two components to a spinning-stretching-setting process using a melt parallel composite spinning device to obtain parallel composite fibers, wherein the spinning-stretching-setting process may adopt a low-speed spinning-high-multiple stretching-setting process, or a high-speed spinning-low-multiple stretching-setting one-step FDY process or a two-step UDY-DT process, wherein the spinning temperature is controlled at 265-295° C., and the spinning speed is controlled at 1000-3000 m / min; subjecting the parallel composite fibers to a wet heat or dry heat treatment again to obtain the two-component composite elastic fiber capable of being dyed at low temperature and normal pressure, wherein the hot water treatment temperature is controlled at 80-100° C., and the elastic elongation of the fiber after the heat treatment is 93-120%, and the elastic recovery rate is 86-94%.
2. The low temperature and normal pressure dyeable bicomponent composite elastic fiber according to claim 1, characterized in that: In the preparation method, the stretching temperature is controlled at 60-100°C, the stretching multiple is 3.8-1.8 times, and the shaping temperature is controlled at 90-170°C.
3. The low temperature and normal pressure dyeable bicomponent composite elastic fiber according to claim 1, characterized in that: The low-temperature and normal-pressure dyeable two-component composite elastic fiber in the preparation method can be dyed to a full color spectrum including black, dark brown, and navy blue using disperse dyes or cationic dyes at normal pressure and low temperature below 100°C, and its color fastness reaches level 4 or above.
4. The low temperature and normal pressure dyeable bicomponent composite elastic fiber according to claim 1, characterized in that: When the cross-sectional structure of the parallel composite fibers in the preparation method is controlled to be a "dumbbell shape", better elasticity can be obtained.
Citation Information
Patent Citations
Side-by-side composite PBT polyester fiber and preparation method thereof
CN106337212A
Production process of PBT / PET (polybutylenes terephthalate / polyethylene terephthalate) double-component elastic composite material
CN107964690A
High and low viscosity PET side-by-side composite self-crimping fibers and preparation method thereof
CN111101237A
New elastic fiber and preparation method thereof
CN101357980A
High-performance polyester composite elastic fiber and manufacturing method thereof
CN101718008A