Environmentally friendly epoxy curing agent and preparation method and application thereof
By using epoxy curing agents prepared by binary primary amines, acrylonitrile, poly primary amines, cyclic carbonates, silane coupling agents and imidazole compounds, the problems of insufficient use and mechanical properties of toxic isocyanates in the prior art are solved. The high mechanical properties of epoxy resin and the development of environmentally friendly epoxy curing agents have been achieved, with a shear strength of more than 10MPa.
Patent Information
- Application Number
- CN202110818781.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-07-20
AI Technical Summary
The existing epoxy resin toughening curing agent uses toxic isocyanate during the preparation process, resulting in high costs and toxic intermediates during the production process. At the same time, its compatibility and mechanical properties with epoxy resin are insufficient, limiting its high-tech end. Application in the field.
Epoxy curing agent prepared by using binary primary amines, acrylonitrile, poly primary amines, cyclic carbonates, silane coupling agents and imidazole compounds, is formed with excellent results by combining the—CN group and the—NHCOO group. A new environmentally friendly epoxy curing agent with mixed effects and flexibility avoids the use of toxic isocyanates and improves the interaction force between the molecular chains through β-OH groups.
The high mechanical properties of the cured epoxy resin products are achieved, and the shear strength reaches more than 10MPa, which significantly improves its performance in mechanical properties and toughness, while avoiding the use of toxic chemicals, which is in line with the concept of green chemistry development.
Smart Images

Figure CN115636922B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of curing agent production, and in particular to an environmentally friendly epoxy curing agent and a preparation method and application thereof. Background Art
[0002] Epoxy resin is a type of thermosetting resin with excellent mechanical properties, chemical resistance and aging resistance, and is widely used in many industries such as aviation, electronics, and construction. However, since the epoxy resin system contains a large number of rigid aromatic structures and has a high cross-linking density, the epoxy resin has poor ability to dissipate external impact and internal stress, which undoubtedly limits its application in high-tech fields. Therefore, it is usually necessary to toughen epoxy resin to improve its comprehensive performance and expand its application field.
[0003] At present, the most commonly used method for toughening epoxy resin is to introduce a toughening agent, such as nitrile rubber (CN109651977A), into the epoxy resin system. Through microphase separation between the toughening agent and the epoxy matrix, crack propagation and plastic deformation are effectively hindered, thereby achieving the purpose of toughening. In addition, the use of thermotropic liquid crystals (CN105754296B) and core-shell structured particles (CN109852003A) can also achieve a significant toughening effect. However, although these methods can have a toughening effect on the epoxy resin matrix, due to the weak interaction between them and the epoxy matrix, they migrate or fail during subsequent use. At the same time, when using these methods to modify epoxy resin, the two need to be mixed evenly first, which undoubtedly brings trouble to the molding process. The use of toughening curing agents can effectively avoid the disadvantages of the above methods. When curing epoxy resin, the soft segment in the curing agent structure can chemically bond to the epoxy system structure and form microphase separation during the curing process, thereby destroying the uniformity of the cross-linked network, promoting stress dispersion in the system, and improving the toughness of the epoxy resin matrix.
[0004] Common toughening curing agents generally contain flexible -NHCOO- groups in their structures. The presence of -NHCOO- groups can give the curing agent excellent properties, but there are also some defects:
[0005] 1) Usually, the synthesis of -NHCOO- groups usually requires the use of toxic isocyanates;
[0006] 2) Isocyanates are expensive and require the use of the toxic “phosgene” method for their preparation;
[0007] 3) Since the -NHCOO- group is a polar group, when the corresponding toughening curing agent is mixed with epoxy resin, the compatibility of the two is affected to a certain extent.
[0008] In the prior art, a Chinese invention patent with publication number CN109486470B discloses an epoxy soybean oil adhesive with imidazole-terminated polyurethane and a preparation method thereof, wherein the imidazole-terminated polyurethane is preferably prepared by using polyether diols, diphenylmethane diisocyanate or hydrogenated diphenylmethane diisocyanate and 2-substituted imidazole compounds with a molecular weight between 106 and 1000 g / mol, and the product molecular weight is between 800 and 4000 g / mol. After the toughening curing agent and epoxy are cured, the corresponding bonding strength is between 2 and 5 MPa. A Chinese patent with publication number CN109355061A discloses a preparation method of a polyurethane-type epoxy curing agent, wherein the curing agent molecule is preferably prepared by using toxic diphenylmethane diisocyanate, polyether diols with a molecular weight between 106 and 1000 g / mol, and a diamine compound containing a primary amino group and a secondary amino group. The molecular weight of the toughening curing agent can reach 8000 g / mol. At the same time, due to the strong polarity of the -NHCOO- group in the polyurethane chain segment, the intermolecular force between the corresponding molecular segments is increased. These factors make the curing agent have a higher viscosity. In addition, the maximum shear strength of the epoxy resin cured product is only 5.04MPa.
[0009] From the statistical analysis of existing patents, it can be seen that although toughening curing agents containing -NHCOO- groups can improve the toughness of epoxy resins to a certain extent, toxic isocyanates are required in the preparation process, and the mechanical strength of the corresponding epoxy resin cured products is greatly lost. Therefore, it is very necessary to develop a new type of environmentally friendly toughening curing agent. On the one hand, it is required to avoid the use of toxic isocyanates and introduce -NHCOO- groups when preparing toughening curing agents; on the other hand, it is required that the toughening curing agent and the epoxy resin cured products have good toughness and mechanical strength. Summary of the invention
[0010] The purpose of the present invention is to provide an environmentally friendly epoxy curing agent and a preparation method thereof, which solves the defects of traditional polyurethane toughened epoxy resins and has the advantages of low viscosity. At the same time, the reaction raw materials do not use toxic isocyanates, avoiding the problems of high cost and toxic intermediates generated during the production process caused by isocyanates. In addition, the introduction of -CN groups can improve the mixing effect between the curing agent and the epoxy resin, and the reaction of cyclic carbonates with amines can introduce -NHCOO- groups into the system structure, and the -OH group at the β position can also improve the interaction between molecular chains. The new environmentally friendly epoxy curing agent can be used in the curing of epoxy resins, and the cured epoxy resin has excellent mechanical properties, and its shear strength can reach more than 10MPa.
[0011] The present invention is achieved through the following technical solutions:
[0012] A novel environmentally friendly epoxy curing agent is prepared from dibasic primary amine, acrylonitrile, polybasic primary amine, cyclic carbonate, silane coupling agent and imidazole compound, and the epoxy curing agent contains the following two structures at the same time:
[0013] .
[0014] Furthermore, the molar ratio of structure (I) to structure (II) is 1:0.1-0.5.
[0015] Furthermore, in the epoxy curing agent, R1 in structure (I) is an alkane segment such as -CH2-, a benzene ring or a cyclohexane structure, and R2 in structure (II) is a polyether segment with a number average molecular weight between 150 and 2500 g / mol.
[0016] A method for preparing the aforementioned epoxy curing agent comprises the following steps:
[0017] a. Take diprimary amine and acrylonitrile at a molar ratio of diprimary amine to acrylonitrile of 1:1~2, and add acrylonitrile dropwise into the diprimary amine at a temperature of 50~90°C for 2~4h to obtain a mixture containing structure (I);
[0018] b. Then weigh the polyamine according to the molar ratio of the diamine to the polyamine of 1:0.5~2, add the polyamine dropwise to the reactant in step a, control the temperature to 70~90°C, stir and mix for 0.5~1.0h to obtain an intermediate;
[0019] c. Then, a cyclic carbonate is selected according to the ratio of functional group n (—NH2): n (cyclic carbonate group) of 1:0.1-0.5, and the cyclic carbonate is added dropwise to the reactant in step b, the temperature is controlled at 70-90° C., and the mixture is stirred for 2-4 hours to obtain an intermediate curing agent containing both structure (I) and structure (II);
[0020] d. Add 0.5% to 2% of the total mass of a silane coupling agent and 1% to 3% of an imidazole compound to step c, mix well, and then discharge to obtain an epoxy curing agent.
[0021] Furthermore, in step a, the diprimary amine is any one or more of an aliphatic diprimary amine, an aromatic diprimary amine and an alicyclic diprimary amine.
[0022] Furthermore, in step b, the polyamine is one or more polyetheramines having a number average molecular weight of 150 to 2500 g / mol.
[0023] Furthermore, in step b, the polyamine is one or more polyetheramines having a number average molecular weight of 200 to 500 g / mol.
[0024] Furthermore, in step c, the cyclic carbonate is one or more of ethylene carbonate, propylene carbonate, glycerol carbonate, ethylene glycol diglycidyl ether type cyclic carbonate, 1,4-butanediol diglycidyl ether type cyclic carbonate, 1,6-hexanediol diglycidyl ether type cyclic carbonate, trimethylolpropane triglycidyl ether type cyclic carbonate and other multifunctional cyclic carbonates.
[0025] Furthermore, in step d, the silane coupling agent is one or more of KH550, KH551, KH580, KH602 and KH792; the imidazole compound is one or more of 2-methylimidazole, 1-benzyl-2-ethylimidazole, 1-aminoethyl-2-methylimidazole or 2-ethyl-4-methylimidazole.
[0026] An application of the novel environmentally friendly epoxy curing agent as mentioned above in epoxy resin curing.
[0027] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0028] 1. In the present invention, an epoxy curing agent is prepared by using diprimary amine, acrylonitrile, polyprimary amine, cyclic carbonate, silane coupling agent and imidazole compound. The epoxy curing agent contains structure (I) and structure (II), that is, it contains -CN group and -NHCOO- group, which can combine the advantages of the two functional groups, give the curing agent excellent mixing effect and flexibility, so that the bonding strength of the cured product of the epoxy curing agent can reach more than 10MPa.
[0029] 2. In the novel environmentally friendly epoxy curing agent prepared in the present invention, there is an -OH group at the β position of the -NHCOO- group in structure (II), which can form a hydrogen bond with the polar group in the curing agent, effectively improving the intermolecular force between the epoxy cured product system, thereby improving its mechanical properties.
[0030] 3. In the present invention, by adopting the preparation method of the epoxy curing agent disclosed in the technical scheme, the synthesis ratio of structure (I) and structure (II) in the epoxy curing agent system can be controlled, and then by adjusting the content ratio of structure (I) and structure (II) in the system, different curing properties can be given to the curing agent, so that the content ratio of structure (I) and structure (II) in the curing agent can be adjusted according to actual needs to obtain epoxy cured products with different properties.
[0031] Fourth, in the present invention, in the synthesis process of the novel epoxy curing agent, the introduction of the -NHCOO- group completely avoids the use of toxic isocyanates, which is in line with the development concept of "green chemistry". BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1It is the infrared spectrum of epoxy curing agent I in Example 1. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0034] Example 1
[0035] This embodiment is a method for preparing a novel environmentally friendly epoxy curing agent, comprising the following steps:
[0036] a) reacting in a molar ratio of 1,6-hexanediamine to acrylonitrile of 1:2, slowly adding acrylonitrile to the fatty amine, controlling the temperature at 70°C, and reacting for 2 h to obtain a mixture containing structure (I);
[0037] b) weighing D230 with a molar ratio of 2 times that of 1,6-hexanediamine, and adding D230 dropwise to the reactant in step a), stirring and mixing at 70°C for 1 hour to obtain an intermediate;
[0038] c) After the mixing is completed, propylene carbonate is added dropwise to the reactants in step b) at a ratio of functional group n (—NH2): n (propylene carbonate group) of 1:0.3, and the mixture is stirred and reacted at 90° C. for 2 h to obtain an intermediate curing agent containing structure (I) and structure (II);
[0039] d) At 70°C, add 1% of the total mass of KH550 and 2% of 2-methylimidazole to step c), mix for 0.5h and then discharge to obtain a novel environmentally friendly epoxy curing agent I. The infrared spectrum of the epoxy curing agent I is shown in the attached figure. Figure 1 shown.
[0040] From the attached Figure 1 It can be seen that 2274cm -1 The infrared absorption peak at position is the vibration peak of -CN group, while 3350cm -1 and 1705cm -1 The absorption peaks at the two positions are attributed to the C=O vibration peaks of the -OH group and the -NHCOO- group, respectively.
[0041] Example 2
[0042] This embodiment is another method for preparing a novel environmentally friendly epoxy curing agent, comprising the following steps:
[0043] a) reacting in a molar ratio of 1,6-hexanediamine to acrylonitrile of 1:1, slowly adding acrylonitrile to the fatty amine, controlling the temperature at 50°C, and reacting for 4 hours to obtain a mixture containing structure (I);
[0044] b) weighing D400 at a molar ratio of 2 times that of 1,6-hexanediamine, and adding D400 dropwise to the reactant in step a), stirring and mixing at 90° C. for 1 h to obtain an intermediate;
[0045] c) After the mixing is completed, propylene carbonate is added dropwise to the reactants in step b) at a ratio of functional group n (NH2): n (propylene carbonate group) of 1:0.5, and the mixture is stirred and reacted at 90° C. for 2 h to obtain an intermediate curing agent containing structure (I) and structure (II);
[0046] d) At 70° C., 1.5% by weight of KH550 and 1.5% by weight of 1-benzyl-2-methylimidazole were added to step c), mixed for 0.5 h, and then discharged to obtain a novel environmentally friendly epoxy curing agent II.
[0047] Example 3
[0048] This embodiment is a method for preparing a novel environmentally friendly epoxy curing agent, comprising the following steps:
[0049] a) reacting in a molar ratio of ethylenediamine to acrylonitrile of 1:2, slowly adding acrylonitrile to the fatty amine, controlling the temperature at 60°C, and reacting for 3 h to obtain a mixture containing structure (I);
[0050] b) Weigh D230 with a molar ratio of 1 to ethylenediamine, add D230 dropwise to the reactant in step a), and stir at 80° C. for 0.8 h to obtain an intermediate;
[0051] c) After the mixing is completed, 1,4-butanediol diglycidyl ether type cyclic carbonate is added dropwise to the reactants in step b) at a ratio of functional group n (-NH2): n (cyclic carbonate group) of 1:0.3, and the mixture is stirred and reacted at 80°C for 3 hours to obtain an intermediate curing agent containing structure (I) and structure (II);
[0052] d) At 70° C., 1.5% by weight of KH580 and 1.5% by weight of 2-methylimidazole were added to step c), mixed for 0.5 h, and then discharged to obtain a novel environmentally friendly epoxy curing agent III.
[0053] Example 4
[0054] This embodiment is a method for preparing a novel environmentally friendly epoxy curing agent, comprising the following steps:
[0055] a) 1,6-hexanediamine and acrylonitrile were taken at a molar ratio of 1:1.5, and acrylonitrile was added dropwise to the dibasic primary amine at 90°C for 2.5 hours to obtain structure (I);
[0056] b) Weigh a mixture of D230 and T403 with a molar ratio of 1.5 times that of 1,6-hexanediamine, wherein the molar ratio of D230 to T403 is 1:1, and add the two polyetheramine mixture dropwise into the reactant in step a), stirring and mixing at 90° C. for 1 hour to obtain an intermediate;
[0057] c) After the mixing is completed, a mixture of 1,6-hexanediol diglycidyl ether type cyclic carbonate and trimethylolpropane triglycidyl ether type cyclic carbonate is added dropwise to the reactants in step b) at a ratio of functional group n (—NH2): n (cyclic carbonate group) of 1:0.4, wherein the molar ratio of the two cyclic carbonates is 1:1, respectively, and the mixture is stirred and reacted at 70° C. for 4 hours to obtain an intermediate curing agent containing structure (I) and structure (II);
[0058] d) At 70° C., 2% by weight of KH550 and 3% by weight of 2-ethyl-4-methylimidazole were added to step c), mixed for 0.5 h, and then discharged to obtain a novel environmentally friendly epoxy curing agent IV.
[0059] Example 5
[0060] This embodiment is a method for preparing a novel environmentally friendly epoxy curing agent, comprising the following steps:
[0061] a) First, 1,4-butanediamine and p-phenylenediamine were weighed and mixed at a molar ratio of 1:1, and then the mixture and acrylonitrile were taken at a molar ratio of 1:1.5, and acrylonitrile was added dropwise to the mixture at a temperature of 90°C and reacted for 3 hours to obtain structure (I);
[0062] b) weighing D2000 at a molar ratio of 0.5 times the above mixture, adding D2000 dropwise into the reactant in step a), stirring and mixing at 90° C. for 0.5 h to obtain an intermediate;
[0063] c) After the mixing is completed, ethylene glycol diglycidyl ether type cyclic carbonate is added dropwise to the reactants in step b) at a ratio of functional group n (-NH2): n (cyclic carbonate group) of 1:0.1, and the mixture is stirred and reacted at 80°C for 3 hours to obtain an intermediate curing agent containing structure (I) and structure (II);
[0064] d) At 70° C., 0.5% by weight of KH551 and 1% by weight of 1-aminoethyl-2-methylimidazole were added to step c), mixed for 0.5 h, and then discharged to obtain a novel environmentally friendly epoxy curing agent V.
[0065] Example 6
[0066] This embodiment is a method for preparing a novel environmentally friendly epoxy curing agent, comprising the following steps:
[0067] a) isophorone diamine and acrylonitrile were prepared in a molar ratio of isophorone diamine to acrylonitrile of 1:1.5, and acrylonitrile was added dropwise to the diprimary amine at 80°C for 4 hours to obtain structure (I);
[0068] b) weighing D400 at a molar ratio of 1.5 times that of isophorone diamine, adding D400 dropwise into the reactant in step a), stirring and mixing at 70° C. for 1 h to obtain an intermediate;
[0069] c) After the mixing is completed, a mixture of ethylene carbonate and 1,4-butanediol diglycidyl ether type cyclic carbonate is added dropwise to the reactants in step b) at a ratio of functional group n (-NH2): n (cyclic carbonate group) of 1:0.5, wherein the molar ratio of the two cyclic carbonates is 1:1, and the mixture is stirred and reacted at 90° C. for 2 hours to obtain an intermediate curing agent containing structure (I) and structure (II);
[0070] d) At 70° C., add 2% by total mass of KH602 and 2% by total mass of 2-ethyl-4-methylimidazole to step 3), mix for 0.5 h, and then discharge the mixture to obtain a novel environmentally friendly epoxy curing agent VI.
[0071] Example 7
[0072] This example is another method for preparing a novel environmentally friendly epoxy curing agent. Compared with Example 1, the difference is that in step a), 1,6-hexanediamine and acrylonitrile are taken at a molar ratio of 1:1, and acrylonitrile is added dropwise to 1,6-hexanediamine at a temperature of 90°C and reacted for 4 hours to obtain structure (I). The remaining steps are the same, and finally a novel environmentally friendly epoxy curing agent VII is obtained.
[0073] Example 8
[0074] This example is another method for preparing a novel environmentally friendly epoxy curing agent. Compared with Example 3, the difference is that in step b), a polyamine is weighed according to the molar ratio of ethylenediamine to D230 of 1:0.5, and the polyamine is added dropwise to the reactant in step a, the temperature is controlled at 90°C, and the mixture is stirred for 0.5h to obtain an intermediate. The remaining steps are the same, and finally a novel environmentally friendly epoxy curing agent VIII is obtained.
[0075] Example 9
[0076] This embodiment is another method for preparing a novel environmentally friendly epoxy curing agent. Compared with Example 5, the difference is that in step c, 1,4-butanediol diglycidyl ether type cyclic carbonate is taken according to the functional group n (-NH2): n (cyclic carbonate group) of 1:0.1, and the cyclic carbonate is added dropwise to the reactant in step b, the temperature is controlled at 70°C, and the mixture is stirred for 4 hours to obtain an intermediate curing agent containing both structure (I) and structure (II). The remaining steps are the same, and finally a novel environmentally friendly epoxy curing agent IX is obtained.
[0077] The new environmentally friendly epoxy curing agent prepared in Examples 1 to 9 was applied to the curing of epoxy resin E51, and the performance of the curing agent and the epoxy cured product was tested. In order to compare the corresponding performance tests of the patent of the present invention, Comparative Example 1 and Comparative Example 2 were added, where Comparative Example 1 was the curing agent 1,6-hexanediamine and Comparative Example 2 was the polyetheramine D230. The specific test standards were as follows:
[0078] Viscosity: in accordance with GB / T 7193-2008 standard;
[0079] Impact strength: in accordance with GB / T 2567-2008 standard;
[0080] Shear strength: in accordance with GB / T 7124-2008 standard, the test tensile rate is 2 mm / min;
[0081] Tensile strength and elongation at break: in accordance with GB / T 2567-2008 standard, the test tensile rate is 10 mm / min;
[0082] Peel strength: The test was carried out in accordance with GB / T2791-1995 standard, and the test tensile rate was 100 mm / min. The properties of epoxy cured products prepared by the epoxy curing agents of various examples are shown in Table 1.
[0083] Table 1:
[0084]
[0085] From Table 1 above, it can be seen that after the epoxy curing agent obtained by the preparation method of the novel environmentally friendly epoxy curing agent disclosed in the present invention reacts with E51, the corresponding cured product has excellent mechanical properties, and its shear strength can be maintained above 10 MPa, and can even reach 30 MPa; the elongation at break can be maintained above 2.5%; the peel strength can reach above 0.8 KN / m, which is significantly higher than the performance of the curing agent in the prior art (such as Comparative Example 1 and Comparative Example 2).
[0086] In the present invention, the diprimary amine may be any one or more of an aliphatic diprimary amine, an aromatic diprimary amine and an alicyclic diprimary amine;
[0087] The types of the aliphatic diprimary amines are ethylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,6-hexanediamine, 1,8-octanediamine, dodecamethylenediamine, dimethyldiaminooctadiene and tetramethyldiaminooctadiene;
[0088] The types of aromatic diprimary amines are p-phenylenediamine, m-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, p-xylene diamine, and m-xylene diamine;
[0089] The types of alicyclic diprimary amines are isophoronediamine, 1,3-bis(aminomethyl)cyclohexane, and 4,4'-diaminodicyclohexylmethane.
[0090] In the present invention, the polyamine is one or more polyetheramines with a number average molecular weight of 150 to 2500 g / mol. The polyetheramines within this molecular weight range have better comprehensive performance. If the molecular weight is too large, such as D2000 with a molecular weight of 2000 g / mol, the prepared curing agent will have too much flexibility, which will have a greater impact on strength.
[0091] In the present invention, the cyclic carbonate is one or more of ethylene carbonate, propylene carbonate, glycerol carbonate, ethylene glycol diglycidyl ether type cyclic carbonate, 1,4-butanediol diglycidyl ether type cyclic carbonate, 1,6-hexanediol diglycidyl ether type cyclic carbonate, trimethylolpropane triglycidyl ether type cyclic carbonate and other multifunctional cyclic carbonates.
[0092] In the present invention, when curing epoxy resin with curing agent, the use of silane coupling agent can improve the wettability and interaction between epoxy resin product and substrate, and can improve shear strength, and the silane coupling agent is one or more of KH550, KH551, KH580, KH602 and KH792. KH550 is preferred, because KH550 is relatively low in price, easy to obtain, and has better effect.
[0093] In the present invention, when the curing agent cures the epoxy resin, the imidazole compound can effectively adjust the reactivity of the curing agent. The imidazole compound is one or more of 2-methylimidazole, 1-benzyl-2-ethylimidazole, 1-aminoethyl-2-methylimidazole or 2-ethyl-4-methylimidazole. 2-methylimidazole and 2-ethyl-4-methylimidazole are preferred, as these two reagents are commonly used, easily available, and inexpensive.
[0094] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention shall fall within the protection scope of the present invention.
Claims
1. An environmentally friendly epoxy curing agent, characterized in that: An epoxy curing agent is prepared by using diprimary amine, acrylonitrile, polyprimary amine, cyclic carbonate, silane coupling agent and imidazole compound, and the epoxy curing agent contains the following two structures at the same time: , The diprimary amine is any one or more of an aliphatic diprimary amine, an aromatic diprimary amine and an alicyclic diprimary amine; The polyvalent primary amine is one or more polyetheramines having a number average molecular weight of 150 to 2500 g / mol; In the epoxy curing agent, R1 in structure (I) is any one or more of the residue of aliphatic diprimary amine, aromatic diprimary amine and alicyclic diprimary amine, and R2 in structure (II) is the residue of a polyetheramine with a number average molecular weight of 150-2500 g / mol.
2. An environmentally friendly epoxy curing agent according to claim 1, characterized in that: The molar ratio of the structure (I) to the structure (II) is 1:0.1-0.
5.
3. A method for preparing the epoxy curing agent according to claim 1, characterized in that: The following steps are involved: a. Take diprimary amine and acrylonitrile at a molar ratio of diprimary amine to acrylonitrile of 1:1~2, and add acrylonitrile dropwise into the diprimary amine at a temperature of 50~90°C for 2~4h to obtain a mixture containing structure (I); b. Then weigh the polyamine according to the molar ratio of the diamine to the polyamine of 1:0.5~2, add the polyamine dropwise to the reactant in step a, control the temperature to 70~90°C, stir and mix for 0.5~1.0h to obtain an intermediate; c. Then, a cyclic carbonate is selected according to the ratio of functional group n (—NH2): n (cyclic carbonate group) of 1:0.1-0.5, and the cyclic carbonate is added dropwise to the reactant in step b, the temperature is controlled at 70-90°C, and the mixture is stirred for 2-4 hours to obtain an intermediate curing agent containing both structure (I) and structure (II); d. Add 0.5% to 2% of the total mass of a silane coupling agent and 1% to 3% of an imidazole compound to step c, mix well, and then discharge to obtain an epoxy curing agent.
4. The method for preparing the epoxy curing agent according to claim 3, characterized in that: In step b, the polyamine is one or more polyetheramines having a number average molecular weight of 200 to 500 g / mol.
5. The method for preparing the epoxy curing agent according to claim 3, characterized in that: In step c, the cyclic carbonate is one or more of ethylene carbonate, propylene carbonate, glycerol carbonate, ethylene glycol diglycidyl ether type cyclic carbonate, 1,4-butanediol diglycidyl ether type cyclic carbonate, 1,6-hexanediol diglycidyl ether type cyclic carbonate, and trimethylolpropane triglycidyl ether type cyclic carbonate.
6. The method for preparing the epoxy curing agent according to claim 3, characterized in that: In step d, the silane coupling agent is one or more of KH550, KH551, KH580, KH602 and KH792; the imidazole compound is one or more of 2-methylimidazole, 1-benzyl-2-ethylimidazole, 1-aminoethyl-2-methylimidazole or 2-ethyl-4-methylimidazole.
7. Use of the environmentally friendly epoxy curing agent according to claim 1 in epoxy resin curing.
Citation Information
Patent Citations
An epoxy resin composition toughened and strengthened by a thermotropic liquid crystal polymer containing an imide structure
CN105754296B
Epoxidized soybean oil adhesive acted by amine harder modified polyurethane and preparation method of epoxidized soybean oil adhesive
CN109355061A
An imidazole-terminated polyurethane epoxy soybean oil adhesive and its preparation method
CN109486470B
Epoxy mono-component structural adhesive and preparation method thereof
CN109651977A
Preparation method of toughened epoxy resin
CN109852003A