A kind of anti-pollution and oxidation-resistant reverse osmosis membrane and its preparation method
By introducing 2-(2,3-epoxypropylthio)thiophene/diglycidyl ether/3,4-diamino-n-(3-trifluoromethyl-phenyl)- The benzenesulfonamide cross-linking functional coating solves the problem of insufficient anti-pollution and oxidation resistance of the reverse osmosis membrane, and significantly improves the anti-pollution, oxidation resistance and flux of the membrane.
Patent Information
- Application Number
- CN202211361827.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-02
AI Technical Summary
The existing reverse osmosis membranes have shortcomings in their anti-pollution and oxidation resistance, especially when maintaining high throughput, it is difficult to effectively improve.
Polymers of 2-(2,3-epoxypropylthio)thiophene/diglycidyl ether/3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonate by introduction of 2-(2,3-epoxypropylthio)thiophene/diglycidyl ether/3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzene Amide cross-linking functional coating, modifying the surface of the reverse osmosis membrane, enhancing its anti-pollution and oxidation resistance.
The reverse osmosis membrane has achieved excellent anti-pollution, oxidation resistance and high throughput, with a bacteriostatic rate of 90%, and significantly improved tolerance and cleaning recovery performance in sodium hypochlorite solution, and reduced flux attenuation to non-modified membranes. 1/3 of that.
Smart Images

Figure BDA0003922296840000061 
Figure BDA0003922296840000062 
Figure BDA0003922296840000081
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water treatment, and in particular to an anti-pollution and oxidation-resistant reverse osmosis membrane and a preparation method and application thereof. Background Art
[0002] Reverse osmosis membranes are widely used in household water purifiers, industrial pure water manufacturing, wastewater treatment and seawater desalination, making important contributions to the sustainable use of water resources. However, in actual use, reverse osmosis membranes still face a series of problems. Among them, membrane pollution and oxidative damage are the challenges faced by reverse osmosis membrane applications.
[0003] In order to slow down membrane pollution, commonly used modification methods include membrane surface coating (for example, the methods disclosed in CN1213985A and CN101450290A), surface chemical modification (the method disclosed in CN104785131), surface grafting (the method disclosed in CN104815567A) and other physical and chemical methods, so as to improve the anti-pollution performance of the reverse osmosis composite membrane by changing the surface hydrophilicity, surface roughness and surface charge of the reverse osmosis membrane.
[0004] In order to improve the oxidation resistance of the reverse osmosis membrane, the currently disclosed patents mainly use two methods: improving the formula of interfacial polymerization film formation or post-treating the polyamide desalination layer. Improved interfacial polycondensation film formation formula technology, such as CN109126486A discloses a method of obtaining a modified aromatic polyamide desalination layer with improved oxidation resistance by doping modified CNO in an aqueous solution. Post-treatment technology for the polyamide desalination layer, such as CN109603587A discloses a method for improving the chlorine resistance of a composite reverse osmosis membrane by soaking the polyamide layer of a polyamide composite reverse osmosis membrane with a sulfur-containing compound solution; in addition, CN108176246A discloses that the oxidation resistance and anti-pollution performance of the reverse osmosis membrane are simultaneously improved by grafting graphene oxide on the surface of a polyamide reverse osmosis membrane.
[0005] Although the prior art has formed some technical solutions for improving the anti-fouling and / or oxidation resistance of reverse osmosis membranes, these technical solutions still need to be further improved in terms of improving the anti-fouling and oxidation resistance of reverse osmosis membranes while maintaining high flux.
[0006] Therefore, there is an urgent need in the art to develop a reverse osmosis membrane with excellent anti-pollution and oxidation resistance as well as high flux. Summary of the invention
[0007] The purpose of the present invention is to provide an anti-pollution, oxidation-resistant reverse osmosis membrane and a preparation method thereof. The present invention introduces a 2-(2,3-epoxypropylthio)thiophene / diglycidyl ether polymer / 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide cross-linked functional coating into the surface of a basic reverse osmosis membrane to prepare a reverse osmosis membrane with excellent anti-pollution, oxidation-resistant performance and high flux.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] A method for preparing an anti-pollution and oxidation-resistant reverse osmosis membrane comprises the following steps:
[0010] 1) contacting the polysulfone-based membrane with an aqueous solution of a multifunctional amine and an oily solution of a multifunctional acyl chloride, respectively, to generate an interfacial polymerization reaction to form a polyamide separation layer, thereby obtaining a basic reverse osmosis membrane;
[0011] 2) An ethanol solution A containing a polymer of 2-(2,3-epoxypropylthio)thiophene and diglycidyl ether and an ethanol solution B containing 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide are mixed and coated on the surface of a basic reverse osmosis membrane and dried.
[0012] The polysulfone-based membrane of the present invention is a polysulfone support membrane formed on a non-woven fabric. The finished product can be directly purchased through commercial channels, or a polysulfone casting solution can be obtained by dissolving a polysulfone resin and ethylene glycol monomethyl ether in dimethylformamide; the polysulfone casting solution after filtration and degassing is then applied to a polyester non-woven fabric, and then put into water to form a membrane through phase conversion, and the polysulfone support membrane is obtained after washing. This is a known technology to those skilled in the art.
[0013] The present invention introduces a cross-linked functional coating of 2-(2,3-epoxypropylthio)thiophene / diglycidyl ether polymer / 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide into the surface of the basic reverse osmosis membrane for modification. Among them, the thiophene group has both antibacterial and antioxidant properties, and the 2-(2,3-epoxypropylthio)thiophene with epoxy group can not only react with the residual amino group on the polyamide membrane surface, but also participate in the cross-linking reaction of the diglycidyl ether polymer and 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide, giving the membrane lasting anti-biological contamination and oxidation resistance. The introduction of fluorinated 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide can effectively reduce the adhesion of pollutants to the reverse osmosis membrane and improve the membrane's anti-pollution and cleaning recovery performance; at the same time, 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide with a diamino group can undergo a cross-linking reaction with a diglycidyl ether polymer to impart durability to the modified product; the presence of sulfonamide effectively mitigates the negative impact of the coating on water production, allowing the membrane to have a higher water flux.
[0014] Further, the polyfunctional amine is a compound having at least two active amino groups, including one or more of an aromatic compound having at least two active amino groups, an aliphatic compound having at least two active amino groups, or an alicyclic compound having at least two active amino groups. Suitable examples include, but are not limited to, one or more of m-phenylenediamine, iso-phenylenediamine, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 2,4-diaminotoluene, 2,6-diaminotoluene, 2,4-diaminoanisyl, amphenol, xylene diamine, ethylene diamine, propylene diamine, tris(2-aminoethyl)amine, 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, piperazine, 2,5-dimethylpiperazine, or 4-aminomethylpiperazine, more preferably m-phenylenediamine.
[0015] Preferably, the mass percentage of the multifunctional amine in the aqueous phase solution of the multifunctional amine is 2.0 wt % to 6.0 wt %.
[0016] Further, the polyfunctional acyl chloride is an acyl halide having at least two functional groups, including one or more of an aromatic acyl halide having at least two functional groups, an aliphatic acyl halide having at least two functional groups, or an alicyclic acyl halide having at least two functional groups. Suitable examples include, but are not limited to, trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride, biphenyl dicarboxylic acid chloride, naphthalene dicarboxylic acid dichloride, benzene trisulfonyl chloride, benzene disulfonyl chloride, monochlorosulfonyl chloride, The invention can be selected from the group consisting of benzene dicarboxylic acid chloride, propane tricarboxylic acid chloride, butane tricarboxylic acid chloride, pentane tricarboxylic acid chloride, glutaryl halide, adipic acid halide, cyclopropane tricarboxylic acid chloride, cyclobutane tetracarboxylic acid chloride, cyclopentane tricarboxylic acid chloride, cyclopentane tetracarboxylic acid chloride, cyclohexane tricarboxylic acid chloride, tetrahydrofuran tetracarboxylic acid chloride, cyclopentane dicarboxylic acid chloride, cyclobutane dicarboxylic acid chloride, cyclohexane dicarboxylic acid chloride and tetrahydrofuran dicarboxylic acid chloride, more preferably trimesoyl chloride.
[0017] Preferably, the mass percentage of the multifunctional acyl chloride in the oil phase solution of the multifunctional acyl chloride is 0.1 wt % to 0.3 wt %.
[0018] Furthermore, the interfacial polymerization reaction time is 10 to 30 seconds.
[0019] Furthermore, in the ethanol A solution of step 2), the concentration of 2-(2,3-epoxypropylthio)thiophene is 0.01 to 1 wt%, preferably 0.1 to 0.3 wt%; the concentration of the diglycidyl ether polymer is 0.01 to 1 wt%, preferably 0.1 to 0.3 wt%.
[0020] The diglycidyl ether polymer of the present invention is preferably one or more of polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, poly(dimethylsiloxane) diglycidyl ether, more preferably polyethylene glycol diglycidyl ether. As a preferred embodiment, the number average molecular weight of the polyethylene glycol diglycidyl ether is 100 to 500,000, preferably 400 to 800, and more preferably 500.
[0021] Furthermore, in the ethanol B solution in step 2), the concentration of 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide is 0.01 to 1 wt %, preferably 0.3 to 0.5 wt %.
[0022] Furthermore, in step 2), the mass ratio of ethanol A solution to ethanol B solution is 1:10 to 10:1, preferably 1:1.
[0023] In step 2) of the present invention, the drying conditions are 60-120° C. for 2-6 minutes.
[0024] The anti-pollution and oxidation-resistant reverse osmosis membrane of the present invention or the reverse osmosis membrane obtained by the preparation method is used as an anti-pollution and oxidation-resistant reverse osmosis membrane in water treatment, especially in water treatment components or devices. The water treatment component or device can be any component or device installed with the anti-pollution and oxidation-resistant polyamide reverse osmosis membrane of the present invention that can be used in the water treatment process. The "applied in a water treatment component or device" includes the component or device product installed with the anti-pollution and oxidation-resistant polyamide reverse osmosis membrane of the present invention, and also includes the product used to prepare such a component or device. The component can be, for example, a spiral membrane component and a disc-tube flat membrane component. The device can be, for example, a household / commercial reverse osmosis water purifier, an industrial boiler feed water reverse osmosis pure water device, an industrial water reuse reverse osmosis device, and a seawater desalination device. The water treatment method can be, for example: drinking water production, wastewater reuse, seawater desalination, beverage concentration, and other methods.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The modified coating provided by the present invention is applied to the reverse osmosis membrane, which can obtain the characteristics of anti-pollution, oxidation resistance and high flux. It is well known in the industry that the culture fluid of Staphylococcus aureus (CFU=10 5 / mL) and cultured at 37℃ for 24h, the antibacterial rate reached 90%; after treating 1000ppm sodium hypochlorite solution for 20h and pH 7.0, the sodium chloride desalination rate can still be maintained in the range of 98.5-99.4%, and the desalination rate reduction rate is ≤1%, even as low as 0.3%, showing better oxidation resistance compared with ordinary reverse osmosis membranes; the flux attenuation amplitude of real water quality continuous operation is reduced to 1 / 3 of that of non-modified membranes, and it shows excellent cleaning recovery performance. Therefore, it can be applied to water treatment fields such as industrial water supply and wastewater reuse.
[0027] (2) The method for preparing the anti-pollution and oxidation-resistant reverse osmosis membrane provided by the present invention improves the tolerance of the reverse osmosis membrane to pollution and oxidizing substances. The preparation method of the present invention has the characteristics of being industrially scalable. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0029] Unless otherwise specified, the raw materials used in the following examples or comparative examples are all commercially available industrial-grade conventional raw materials. The main raw material information is shown in Table 1 below.
[0030] Table 1 Raw materials
[0031]
[0032] Performance testing method:
[0033] 1. Evaluation of salt rejection and permeate flux
[0034] Salt rejection rate and permeation flux are two important parameters for evaluating the separation performance of reverse osmosis membranes. The present invention evaluates the separation performance of reverse osmosis membranes according to GB / T32373-2015 "Test Method for Reverse Osmosis Membrane".
[0035] The desalination rate (R) is defined as: under certain operating conditions, the salt concentration of the feed solution (C f ) and the salt concentration in the permeate (C p ) and then divided by the feed solution salt concentration (C f ), as shown in formula (1).
[0036]
[0037] Permeation flux is defined as the volume of water that passes through a unit membrane area per unit time under certain operating conditions, and its unit is L / (m 2 h).
[0038] The operating conditions used in the reverse osmosis membrane performance measurement in the present invention are: the feed liquid is a 2000 ppm sodium chloride aqueous solution, the solution pH is 7.5±0.5, the operating pressure is 1.55 MPa, and the operating temperature is 25°C.
[0039] 2. Evaluation of anti-pollution performance
[0040] 2.1 Flux decay and recovery rate in pollution
[0041] First, the initial permeation flux of the membrane was tested at 25°C and 1.1MPa using wastewater with COD 70mg / L, pH=6.4, conductivity 3200mg / L, and total bacterial count 7000CFU / ml as raw water. After 24 hours of continuous operation, the permeation flux of the membrane after contamination was tested. Flux attenuation rate = 1-(permeation flux after contamination / initial permeation flux).
[0042] After the pollution is over, switch to pure water to clean the polluted membrane in situ for 30 minutes, and then switch to wastewater raw water to measure the permeation flux of the reverse osmosis membrane, which is recorded as the permeation flux after cleaning. Flux recovery rate = permeation flux after cleaning / initial permeation flux.
[0043] 2.2 Antibacterial rate
[0044] After the membranes were sterilized by ultraviolet irradiation, they were immersed in Staphylococcus aureus culture medium (CFU = 10 5 / mL), cultured at 37°C for 24h, measured the number of bacteria or colonies and calculated the percentage of bacteria or colonies reduction R, the calculation formula is as follows:
[0045] R(%)=100%×(AB) / A
[0046] Where A is the number of bacteria or colonies on the basic reverse osmosis membrane, and B is the number of bacteria or colonies on the membrane after coating modification;
[0047] 3. Evaluation of oxidation resistance
[0048] A sodium hypochlorite solution with a concentration of 1000ppm was prepared, and its pH value was adjusted to 7.0 with 1mol / L hydrochloric acid. The reverse osmosis membranes prepared in the following comparative examples and examples were immersed in the sodium hypochlorite solution for 20 hours, and then the membranes were taken out and the membrane surface was repeatedly rinsed with deionized water. Subsequently, the membranes were immersed in a sodium bisulfite aqueous solution with a mass concentration of 0.1wt% to remove residual active chlorine. After rinsing the membrane surface with deionized water, the membranes were immersed in deionized water for 2 hours and then their desalination rate and permeation flux were tested.
[0049] Example 1
[0050] Step 1)
[0051] Preparation of polysulfone support membrane: 250g of polysulfone casting solution containing 16.5wt% polysulfone resin is prepared in N,N-dimethylformamide; then the polysulfone casting solution after filtration and degassing is scraped on a polyester non-woven fabric; then it is put into water to form a membrane through phase conversion, and then washed to obtain a polysulfone support membrane.
[0052] Preparation of basic reverse osmosis membrane: first prepare a 3wt% aqueous solution of m-phenylenediamine, then immerse the wet polysulfone support membrane in the aqueous solution to remove excess water on the surface; then contact it with a 0.12wt% organic solution of trimesoyl chloride for 40s to form a polyamide composite membrane through interfacial polycondensation; and soak the obtained cross-linked aromatic polyamide reverse osmosis membrane in a 5wt% aqueous solution of glycerol for standby use.
[0053] Step 2)
[0054] Prepare an ethanol solution of 0.1wt% 2-(2,3-epoxypropylthio)thiophene and 0.1wt% polyethylene glycol diglycidyl ether, stir at room temperature for 2h until uniform, and obtain solution A. Then, prepare an ethanol solution of 0.3wt% 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide, stir at room temperature for 2h until uniform, and obtain solution B. After mixing solutions A and B in a mass ratio of 1:1, apply them on the surface of the basic reverse osmosis membrane, and dry them at 70℃ for 6min to obtain a reverse osmosis membrane with both anti-pollution and oxidation resistance.
[0055] Embodiments 2 to 5
[0056] The reverse osmosis membranes in Examples 2 to 5 were prepared respectively according to the same method as Example 1, except that the amounts of raw materials added in Table 1 were different.
[0057] Comparative Examples 1 to 6
[0058] The reverse osmosis membranes in Comparative Examples 1 to 6 were prepared respectively in the same manner as in Example 1, except that the amounts of raw materials added in Table 2 were different.
[0059] Table 2 Components and process conditions of the embodiments and comparative examples
[0060]
[0061] The reverse osmosis membranes obtained in different embodiments and comparative examples were evaluated for their salt rejection rate, permeation flux, anti-fouling and oxidation resistance. The results are listed in Table 3.
[0062] Table 3 Evaluation results of embodiments and comparative examples
[0063]
[0064] It can be seen from the above test results that the reverse osmosis membrane with the cross-linked functional coating of 2-(2,3-epoxypropylthio)thiophene / polyethylene glycol diglycidyl ether / 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide of the present invention has more durable and excellent anti-pollution performance, oxidation resistance and high flux, can resist oxide damage and biological contamination in wastewater, and is easier to clean and restore membrane flux.
[0065] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing an anti-pollution and oxidation-resistant reverse osmosis membrane, comprising the following steps: 1) contacting the polysulfone-based membrane with an aqueous solution of a multifunctional amine and an oily solution of a multifunctional acyl chloride, respectively, to generate an interfacial polymerization reaction to form a polyamide separation layer, thereby obtaining a basic reverse osmosis membrane; 2) An ethanol solution A containing a polymer of 2-(2,3-epoxypropylthio)thiophene and diglycidyl ether and an ethanol solution B containing 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide are mixed and coated on the surface of a basic reverse osmosis membrane and dried.
2. The method according to claim 1, characterized in that: The polyfunctional amine is a compound having at least two active amino groups.
3. The method according to claim 1, characterized in that The multifunctional amine is one or more of an aromatic compound having at least two active amino groups, an aliphatic compound having at least two active amino groups, or an alicyclic compound having at least two active amino groups.
4. The method according to claim 1, characterized in that: The multifunctional amine is one or more of m-phenylenediamine, iso-phenylenediamine, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 2,4-diaminotoluene, 2,6-diaminotoluene, 2,4-diaminoanisyl, amphenol, xylene diamine, ethylene diamine, propylene diamine, tris(2-aminoethyl)amine, 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, piperazine, 2,5-dimethylpiperazine or 4-aminomethylpiperazine.
5. The method according to claim 1, characterized in that The polyfunctional acid chloride is an acid halide having at least two functional groups.
6. The method according to claim 1, characterized in that The multifunctional acyl chloride is one or more of an aromatic acyl halide having at least two functional groups, an aliphatic acyl halide having at least two functional groups, or an alicyclic acyl halide having at least two functional groups.
7. The method according to claim 1, characterized in that The multifunctional acid chloride is one or more of trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride, biphenyl dicarboxylic acid chloride, naphthalene dicarboxylic acid dichloride, benzene trisulfonyl chloride, benzene disulfonyl chloride, monochlorosulfonylbenzene dicarboxylic acid chloride, propane tricarboxylic acid chloride, butane tricarboxylic acid chloride, pentane tricarboxylic acid chloride, glutaryl halide, adipic acid halide, cyclopropane tricarboxylic acid chloride, cyclobutane tetracarboxylic acid chloride, cyclopentane tricarboxylic acid chloride, cyclopentane tetracarboxylic acid chloride, cyclohexane tricarboxylic acid chloride, tetrahydrofuran tetracarboxylic acid chloride, cyclopentane dicarboxylic acid chloride, cyclobutane dicarboxylic acid chloride, cyclohexane dicarboxylic acid chloride or tetrahydrofuran dicarboxylic acid chloride.
8. The method according to claim 1, characterized in that The mass percentage of the multifunctional acyl chloride in the oil phase solution of the multifunctional acyl chloride is 0.1 wt % to 0.3 wt %, and the mass percentage of the multifunctional amine in the water phase solution of the multifunctional amine is 2.0 wt % to 6.0 wt %.
9. The method according to claim 1, characterized in that: Step 2) In the ethanol A solution, the concentration of 2-(2,3-epoxypropylthio)thiophene is 0.01 to 1 wt%.
10. The method according to claim 1, characterized in that Step 2) In the ethanol A solution, the concentration of 2-(2,3-epoxypropylthio)thiophene is 0.1-0.3 wt%.
11. The method according to claim 1, characterized in that: Step 2) In the ethanol A solution, the concentration of the diglycidyl ether polymer is 0.01-1 wt%.
12. The method according to claim 1, characterized in that Step 2) In the ethanol A solution, the concentration of the diglycidyl ether polymer is 0.1-0.3 wt%.
13. The method according to claim 1, characterized in that The diglycidyl ether polymer comprises one or more of polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and poly(dimethylsiloxane) diglycidyl ether.
14. The method according to claim 13, characterized in that The number average molecular weight of the polyethylene glycol diglycidyl ether is 100,000 to 500,000.
15. The method according to claim 13, characterized in that The number average molecular weight of the polyethylene glycol diglycidyl ether is 500.
16. The method according to claim 1, characterized in that In the ethanol B solution in step 2), the concentration of 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide is 0.01-1 wt%.
17. The method according to claim 1, characterized in that In the ethanol B solution in step 2), the concentration of 3,4-diamino-n-(3-trifluoromethyl-phenyl)-benzenesulfonamide is 0.3-0.5 wt %.
18. The method according to claim 1, characterized in that In step 2), the mass ratio of ethanol A solution to ethanol B solution is 1:10 to 10:
1.
19. A pollution-resistant and oxidation-resistant reverse osmosis membrane prepared according to the method according to any one of claims 1 to 18.