A bimetallic single-atom carbon-based catalyst, preparation method and application thereof

By designing bimetallic single atom carbon-based catalyst, the problems of harsh catalytic conditions and the use of cocatalysts in the Sonogashira coupling reaction are solved, and the catalytic effect with high activity and high selectivity under mild conditions is achieved. It is suitable for a variety of halogenated benzene The coupling reaction is in line with the concept of green chemistry and atomic economics.

CN115672373BActive Publication Date: 2024-11-26BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211334223.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-11-26
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

The catalytic conditions in the Sonogashira coupling reaction are harsh and cocatalysts are needed. The existing catalysts are not universal for activation of different halogen substituted substrates, making it difficult to achieve high activity and selectivity under mild conditions.

Method used

Carbon-based catalysts using bimetallic single atoms, including carbon-doped nitrogen support, support palladium and copper, the atomic ratio of palladium and copper is 0.1-1:0.1-1, with an average spacing of 2.5-4.5 Angstroms. By adjusting the proportion of metal precursors Doping with N in carbon materials, a catalyst with a dual active center is designed to achieve high selectivity and universality of reactants.

Benefits of technology

High activity and high selectivity under low temperature and normal pressure without a promoter, reduce the amount of precious metals, and widely applicable, avoid substrate self-coupling. It is suitable for a variety of substituted substrates, and conforms to the concept of green chemistry and atomic economics. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115672373B_ABST
    Figure CN115672373B_ABST
Patent Text Reader

Abstract

The present invention discloses a carbon-based catalyst of a bimetallic single atom, a preparation method and an application thereof, wherein the carbon-based catalyst comprises a carbon-based carrier, wherein the carrier carries two metal single atoms of palladium and copper, wherein the atomic ratio of palladium to copper is 0.1-1:0.1-1, and the average spacing between the palladium and copper atoms is 2.5-4.5 angstroms. The preparation method of the bimetallic single-atom catalytic material of the present invention is simple, and the bimetallic single atoms of Pd and Cu are used as reactive substances, and hollow nanospheres of nitrogen-doped carbon are used as carriers, and the structure is stable and the catalytic activity is high. The Sonogashira coupling reaction catalyzed by the catalytic material prepared by the present invention has mild conditions, and there is no need to add expensive and difficult-to-dissolve co-catalysts, and good catalytic activity is also shown for chlorobenzene that is difficult to be activated. It is a preparation method that complies with green chemistry and atom economy and has industrial synthesis value, and has achieved good technical effects, and provides a unique idea for the design of heterogeneous catalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material preparation and catalysis, and in particular to a bimetallic single-atom carbon-based catalyst, a preparation method and application thereof. Background Art

[0002] Sonogashira coupling reaction can achieve Csp 2 Cross-coupling with Csp is one of the effective means to construct carbon-carbon triple bonds, and it plays an important role in the field of organic total synthesis and industrial production. Traditional homogeneous catalysts rely on complex and toxic organophosphine ligands, and the cost and recyclability of the catalyst have always been a difficult problem to solve. The existing heterogeneous catalysts have insufficient intrinsic activity, and additional insoluble and expensive co-catalysts are required to improve the reaction selectivity. The reaction often requires higher temperatures (such as 140°C) and longer reaction times (such as 10h); the amount of precious metals used is large, and the catalyst cost is high. Moreover, the system often has side reactions and by-products such as self-coupling of substrate molecules, and there is a problem of insufficient catalyst selectivity. In addition, it is worth noting that the different substrate substituents in the system often lead to different degrees of difficulty in the reaction. Compared with the coupling reaction of iodobenzene and phenylacetylene, it is more difficult to activate bromobenzene, especially chlorobenzene, and participate in the coupling reaction. Most of the catalysts reported so far can only catalyze the coupling reaction in the presence of iodobenzene, and do not have good universality for the activation of different halogen-substituted substrates. Therefore, it is particularly important to explore a catalyst that can ensure both reaction activity and selectivity under relatively mild reaction conditions for the Sonogashira coupling reaction.

[0003] As a bridge between homogeneous catalysis and heterogeneous catalysis, single-atom catalysts are highly active, green, atom-economical and easily recyclable, and are strong contenders for ideal catalysts. In addition, compared with metal single-atom catalysts, bimetallic single-atom catalysts have dual active centers. The present invention proposes that the two reactants can be adsorbed on different atoms to react, and the spatial distribution and electronic structure of the two active sites can be regulated by adjusting the ratio of metal precursor salts, thereby effectively regulating the bimolecular reaction process in the Sonogashira coupling reaction, which can significantly improve the selectivity and universality of the reaction. Summary of the invention

[0004] One of the problems to be solved by the present invention is to solve the problem that the catalytic conditions in the current Sonogashira coupling reaction are harsh and a co-catalyst is required, and to provide a new catalyst and a synthesis method thereof. In order to solve the above technical problems, the present invention intends to adopt the following technical solutions:

[0005] The present invention relates to a carbon-based catalyst of a double metal single atom, the carbon-based catalyst comprises a carbon-doped nitrogen carrier, the carrier carries two metal single atoms of palladium and copper, the atomic ratio of palladium and copper is 0.1-1:0.1-1, and the average distance between the palladium and copper atoms is 2.5-4.5 angstroms; preferably 2.5-3.5 angstroms. The present invention creatively finds that when the atomic ratio of Cu and Pd is close to 1:1, the number of double single atom pairs formed is the largest and the average distance between the two meets the distance required for the coupling reaction (i.e., 2.5-4.5 angstroms, preferably 2.5-3.5 angstroms), thereby increasing the probability of cross-coupling of the two reactants, effectively avoiding the self-coupling phenomenon of the substrate molecule, thereby improving the selectivity of the target product, and having good tolerance to substrate molecules with a variety of different substituents, and can realize the diversified synthesis of a variety of important compounds. The two active sites respectively adsorb and activate the two reaction substrates, so that the reaction can be highly active and highly selectively converted under green conditions such as low temperature, normal pressure, and no catalyst, and has a high catalytic activity for the difficult-to-activate reactant substrates bromobenzene and chlorobenzene. Compared with the prior art, the present invention has the advantages of mild reaction conditions, convenient operation, simple process, cheap and easy-to-obtain raw materials, wide applicability, and reusability. The amount of precious metals used is reduced by 1 to 3 orders of magnitude (compared with ACS Appl. Meter. Interfaces 2015, 7, 3199-3206 and other series of results), high utilization rate of precious metals and high catalytic activity, which conforms to the concept of green chemistry and atomic economy. Moreover, the heterogeneous catalytic system does not need to add difficult-to-dissolve and expensive organic homogeneous catalysts, avoiding the problems of organic catalysts, additives, etc. and the difficulty of product separation and purification.

[0006] In a preferred embodiment of the present invention, the atomic ratio of palladium to copper is 0.5-1:0.5-1; preferably 0.7-1:0.7-1; and more preferably 0.9-1:0.9-1. The present invention creatively discovered that when the atomic ratio of copper and palladium is close to 1:1, the number of double single atom pairs formed is the largest and the average distance between the two meets the distance required for the coupling reaction.

[0007] In a preferred embodiment of the present invention, the carbon-based carrier is a carbon-nitrogen material. Nitrogen doping helps to anchor metal sites, and the performance of ordinary commercial carbon-based carriers is not as good as this. The present invention is more conducive to controlling the spacing of active sites and achieving a significant improvement in the selectivity of the Sonogashira coupling reaction by regulating the feed ratio of metal precursor salts and the strategy of incorporating N into carbon materials as coordination anchoring sites, which provides a unique idea for the design of heterogeneous catalysts and provides new materials and new methods for organic synthesis reactions.

[0008] In a preferred embodiment of the present invention, the ratio of the weight of the carbon-based carrier to the sum of the weights of palladium and copper is 62500-45454:1-2. The present invention can significantly reduce the metal content, while ensuring the catalytic activity, and can also effectively reduce the cost of the catalyst.

[0009] Another aspect of the present invention relates to a method for preparing the above-mentioned carbon-based catalyst, which comprises the following steps:

[0010] a. Styrene, surfactant and thermal initiator are placed in deionized water, heated and stirred, cooled, and the resulting precipitate is dispersed in a polar solvent after centrifugal washing;

[0011] b. Using the precipitate obtained in step a as a template, adding small molecular carbon nitrogen compounds and palladium and copper precursor salts to a buffer solution with a pH of 7-10, centrifuging, washing and drying to obtain a catalyst precursor;

[0012] c. The product obtained in step b is calcined at 700-900°C to obtain a powdered sample; if the calcination temperature is too low, the PS sphere precursor is not calcined completely, resulting in residual impurities; if the calcination temperature is too high, the morphology of the carbon sphere will collapse, resulting in the embedding of the catalytic active sites.

[0013] d. The powdered sample obtained in step c is treated with acid, centrifuged, washed and dried to obtain a double single-atom catalyst.

[0014] Preferably, the surfactant described in step a includes but is not limited to cetyltrimethylammonium bromide (CTAB), cetyltrimethylammonium chloride (CTAC), polyvinylpyrrolidone (PVP) and sodium dodecylbenzene sulfonate (SDBS).

[0015] Preferably, the thermal initiator described in step a includes but is not limited to inorganic peroxide initiators, such as potassium persulfate, sodium persulfate and ammonium persulfate.

[0016] Preferably, the polar solvent described in step a includes but is not limited to methanol, ethanol, ethylene glycol, isopropanol and water.

[0017] Preferably, the metal copper salt described in step b includes but is not limited to inorganic or organic metal copper salts, such as copper nitrate, copper acetate, copper chloride, copper sulfate, copper acetylacetonate and copper phthalocyanine.

[0018] Preferably, the metal palladium salt in step b includes but is not limited to inorganic or organic metal copper salts, palladium acetylacetonate, palladium sulfate and palladium chloride.

[0019] Preferably, the small molecule carbon-nitrogen compound described in step b includes, but is not limited to, melamine, dicyandiamide, pyridine, urea and cyanoguanidine.

[0020] Preferably, the drying temperature in step b is 30-100° C. and the drying time is 4-24 h.

[0021] Preferably, the pH adjuster in step b is one or more of hydrochloric acid, sulfuric acid, nitric acid, sodium hydroxide, sodium carbonate and sodium bicarbonate.

[0022] Preferably, the calcination temperature and time in step c are 0.5-10 h, the heating rate is 2-10° C. / min, and the calcination atmosphere is one of argon, helium, air and nitrogen.

[0023] Preferably, the acid in step d is a diluted acid, including but not limited to hydrochloric acid, the acid treatment temperature is 50-100°C, the time is 2-48h, and the drying temperature is 30-100°C, and the time is 4-24h.

[0024] Another aspect of the present invention relates to the use of the above catalyst in catalyzing the coupling reaction of phenylacetylene and halogenated benzene, characterized in that the amount of the catalyst used in the reaction is 1%-3% of the mass of the reactants, the reaction temperature is 70-140°C, the reaction pressure is normal pressure but not limited to normal pressure, and the reaction time is 4-24h. Preferably, the reaction solvent is ethanol, which has a higher reaction selectivity than other solvents (such as toluene, DMF). It should be particularly noted that although the reaction pressure of the present invention is not limited to normal pressure, surprisingly, the catalyst of the present invention can achieve high catalytic activity under normal pressure.

[0025] In a preferred embodiment of the present invention, the catalytic conversion rate of the reaction is above 98%, and the selectivity of the reaction is above 92%, preferably above 94%.

[0026] In a preferred embodiment of the present invention, the halogenated benzene is selected from one or a combination of two or more of iodobenzene, chlorobenzene and bromobenzene.

[0027] Beneficial results of the present invention:

[0028] The present invention combines the template method, the wet impregnation method and the high-temperature calcination method to prepare a supported catalyst with a close-coordinated double single-atom structure. By regulating the feed ratio of the two metal precursors, the number of double single-atom pairs and the metal spacing in the catalyst are different, and the two metal active sites are effectively regulated, which significantly improves the selectivity of the catalytic Sonogashira coupling reaction. Compared with the existing technology, the preparation method of the double single-atom catalytic material described in the present invention is simple, the structure is stable, the catalytic activity is high, and the amount of Pd is two orders of magnitude less. The Sonogashira coupling reaction catalyzed by the catalytic material prepared by the present invention is mild, and there is no need to add expensive and difficult to dissolve co-catalysts, and for chlorobenzene that is difficult to be activated, it also shows good catalytic activity. It is a preparation method that conforms to green chemistry and atom economy and has industrial synthesis value, and has achieved good technical effects, and provides a unique idea for the design of heterogeneous catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 : Reaction equation of Sonogashira coupling reaction.

[0030] Figure 2 : Pd prepared in Example 1 54 Cu 46 Transmission electron microscopy image of the / CN double single-atom catalyst.

[0031] Figure 3 : Pd prepared in Example 1 54 Cu 46 Spherical aberration-corrected high-resolution transmission electron microscopy image of the / CN double single-atom catalyst.

[0032] Figure 4 : Pd prepared in Example 1 54 Cu 46 / CN double single atom catalyst.

[0033] Figure 5 : Pd prepared in Example 2 86 Cu 14 / CN catalyst has a distance between two metal atoms.

[0034] Figure 6 : Pd prepared in Example 3 37 Cu 63 / CN double single atom catalyst.

[0035] Figure 7 : Transmission electron microscopy image of the Cu / CN single atom catalyst prepared in Comparative Example 1.

[0036] Figure 8: Transmission electron microscopy image of the Pd / CN single atom catalyst prepared in Comparative Example 2.

[0037] Fig. 9 : Transmission electron microscopy image of the PdCu alloy nanocatalyst prepared in Comparative Example 4.

[0038] Fig.10 : X-ray diffraction patterns of the Cu / CN and Pd / CN single atom catalysts prepared in Comparative Examples 1 and 2.

[0039] Fig.11 : X-ray diffraction pattern of the PdCu alloy nanocatalyst prepared in Comparative Example 3.

[0040] Fig.12 : Schematic diagram of synchronous fluorescence detection of the catalytic reaction in Example 4, wherein: (a) Pd 54 Cu 46 / CN catalytic reaction; (b) synchronous fluorescence spectrum of the mixture after reaction; (b) synchronous fluorescence spectrum of the mixture of phenylacetylene and diphenylacetylene with different concentrations (black line: 0.2mmol / L, red line: 0.3mmol / L, blue line: 0.4mmol / L, green line: 0.5mmol / L and purple: 0.6mmol / L); (c) standard curve of the reactant phenylacetylene; (d) standard curve of the target product diphenylacetylene. DETAILED DESCRIPTION

[0041] Example 1

[0042] a. Dissolve 1.5 g PVP in deionized water, then add styrene and 110 mg ammonium persulfate, stir in an oil bath at 70 ° C for 4 h, cool, wash and centrifuge, and the resulting PS sphere precipitate is dispersed in a polar solvent;

[0043] b. First, use a pipette to take the precipitate dispersion obtained in step a, disperse it in a flask with deionized water to obtain dispersion 1, dissolve 80 mg of dopamine hydrochloride and 15 mg of urea in a buffer solution, and add them to the dispersion 1 just obtained to obtain dispersion 2, weigh 0.002 mmol of sodium chloropalladate and 0.0105 mmol of copper chloride, dissolve them, add them to dispersion 2, stir at room temperature for 24 hours, wash with anhydrous ethanol and dry;

[0044] c. The dried precipitate was transferred to a porcelain boat, placed in a N2 atmosphere, heated to 800°C and calcined for 2h to obtain PdCu NPs / CN material;

[0045] d. Place the PdCu NPs / CN material obtained in step c into a sample bottle, add dilute nitric acid solution, and place the sample bottle in a heating module at 80°C for 24 hours to remove substances in other forms of the two metals, such as metal oxides, metal nanoparticles, etc., to ensure that the two metals exist in the form of single atoms. After completion, centrifuge and wash with anhydrous ethanol and deionized water to obtain Pd 54 Cu 46 / CN double single atom catalyst (Pd:Cu=54:46 atomic ratio).

[0046] Example 2

[0047] a. Dissolve 1.5 g PVP in deionized water, then add styrene and 110 mg ammonium persulfate, stir in an oil bath at 70 ° C for 4 h, cool, wash and centrifuge, and the resulting PS sphere precipitate is dispersed in a polar solvent;

[0048] b. First, use a pipette to take the precipitate dispersion obtained in step a, disperse it in a flask with deionized water to obtain dispersion 1, dissolve 80 mg of dopamine hydrochloride and 15 mg of urea in a buffer solution, and add them to the dispersion 1 just obtained to obtain dispersion 2, weigh 0.0035 mmol of sodium chloropalladate and 0.0035 mmol of copper chloride, dissolve them, add them to dispersion 2, stir at room temperature for 24 hours, wash with anhydrous ethanol and dry;

[0049] c. The dried precipitate was transferred to a porcelain boat, placed in a N2 atmosphere, heated to 800°C and calcined for 2h to obtain PdCu NPs / CN material;

[0050] d. Place the PdCu NPs / CN material obtained in step c into a sample bottle, add dilute nitric acid solution, and place the sample bottle in a heating module at 80°C for 24 hours to remove substances in other forms of the two metals, such as metal oxides, metal nanoparticles, etc., to ensure that the two metals exist in the form of single atoms. After completion, centrifuge and wash with anhydrous ethanol and deionized water to obtain Pd 86 Cu 14 / CN double single atom catalyst.

[0051] Example 3

[0052] a. Dissolve 1.5 g of PVP in deionized water, then add styrene and 110 mg of ammonium persulfate, stir in an oil bath at 70 ° C for 4 h, cool, wash and centrifuge, and the resulting PS sphere precipitate is dispersed in a polar protic solvent;

[0053] b. First, use a pipette to take the precipitate dispersion obtained in step a, disperse it in a flask with deionized water to obtain dispersion 1, dissolve 80 mg of dopamine hydrochloride and 15 mg of urea in a buffer solution, and add them to the dispersion 1 just obtained to obtain dispersion 2, weigh 0.0015 mmol of sodium chloropalladate and 0.0015 mmol of copper chloride, dissolve them, add them to dispersion 2, stir at room temperature for 24 hours, wash with anhydrous ethanol and dry;

[0054] c. The dried precipitate was transferred to a porcelain boat, placed in a N2 atmosphere, heated to 800°C and calcined for 2h to obtain PdCu NPs / CN material;

[0055] d. The PdCu NPs / CN material obtained in step c was placed in a sample bottle, a dilute nitric acid solution was added, and the sample bottle was placed in a heating module for heat treatment at 80°C for 24 hours to remove substances in other forms of the two metals, such as metal oxides, metal nanoparticles, etc., to ensure that the two metals exist in the form of single atoms. After completion, the PdCu NPs / CN material was centrifuged and washed with anhydrous ethanol and deionized water to obtain 37 Cu 63 / CN double single atom catalyst.

[0056] Comparative Example 1

[0057] a. Dissolve 1.5 g of PVP in deionized water, then add styrene and 110 mg of ammonium persulfate, stir in an oil bath at 70 ° C for 4 h, cool, wash and centrifuge, and the resulting PS sphere precipitate is dispersed in a polar protic solvent;

[0058] b. First, use a pipette to take the precipitate dispersion obtained in step a, disperse it in a flask with deionized water to obtain dispersion 1, dissolve 80 mg of dopamine hydrochloride and 15 mg of urea in a buffer solution, and add them to the dispersion 1 just obtained to obtain dispersion 2, weigh 0.007 mmol of copper chloride, dissolve it and add it to dispersion 2, stir at room temperature for 24 hours, wash with anhydrous ethanol and dry;

[0059] c. The dried precipitate was transferred to a porcelain boat, placed in a N2 atmosphere, heated to 800°C and calcined for 2 h to obtain a CuNPs / CN single atom catalyst;

[0060] d. Place the Cu NPs / CN material obtained in step c into a sample bottle, add dilute nitric acid solution, and place the sample bottle in a heating module for heat treatment at 80°C for 24 hours to remove substances in other forms of the two metals, such as metal oxides, metal nanoparticles, etc., to ensure that the two metals exist in the form of single atoms. After completion, centrifuge and wash with anhydrous ethanol and deionized water to obtain a Cu / CN single atom catalyst.

[0061] Comparative Example 2

[0062] a. 1.5 g PVP was dissolved in deionized water, followed by the addition of styrene and 110 mg ammonium persulfate, stirred in an oil bath at 70 ° C for 4 h, cooled, washed and centrifuged, and the obtained PS sphere precipitate was dispersed in the obtained precipitate dispersed in a polar protic solvent;

[0063] b. First, use a pipette to take the precipitate dispersion obtained in step a, centrifuge and disperse it in a flask with deionized water to obtain dispersion 1, dissolve 80 mg of dopamine hydrochloride and 15 mg of urea in a buffer solution, and add them to the dispersion 1 just obtained to obtain dispersion 2, weigh 0.007 mmol of sodium chloropalladate, dissolve it and add it to dispersion 2, stir at room temperature for 24 hours, wash with anhydrous ethanol and dry;

[0064] c. The dried precipitate was transferred to a porcelain boat, placed in a N2 atmosphere, heated to 800°C and calcined for 2h to obtain PdNPs / CN material;

[0065] d. Place the Pd NPs / CN obtained in step c into a sample bottle, add dilute nitric acid solution, and place the sample bottle in a heating module for heat treatment at 80°C for 24 hours to remove substances in other forms of the two metals, such as metal oxides, metal nanoparticles, etc., to ensure that the two metals exist in the form of single atoms. After completion, the Pd / CN single atom catalyst is obtained by centrifugation washing with anhydrous ethanol and deionized water.

[0066] Comparative Example 3

[0067] The materials synthesized in Comparative Example 1 and Comparative Example 2 are mixed in a ratio of 1:1 to obtain a mixture.

[0068] Comparative Example 4

[0069] a. Dissolve 1.5 g of PVP in deionized water, then add styrene and 110 mg of ammonium persulfate, stir in an oil bath at 70 ° C for 4 h, cool, wash and centrifuge, and the resulting PS sphere precipitate is dispersed in a polar protic solvent;

[0070] b. First, use a pipette to take the precipitate dispersion obtained in step a, centrifuge and disperse it in a flask with deionized water to obtain dispersion 1, dissolve 80 mg of dopamine hydrochloride and 15 mg of urea in a buffer solution, and add them to the dispersion 1 just obtained to obtain dispersion 2, weigh 0.002 mmol and 0.0105 mmol of the two metals respectively, add them to the dispersion 2 after dissolution, stir at room temperature for 24 hours, wash with anhydrous ethanol and dry;

[0071] c. The dried precipitate was transferred to a porcelain boat, placed in a N2 atmosphere, heated to 800°C and calcined for 2h to obtain a PdCu alloy nanocatalyst.

[0072] Example 4

[0073] 20 mg of Pd 54 Cu 46 / CN double single atom catalyst and stirrer were placed in a reaction tube, 10mL ethanol, 0.5mmol iodobenzene, 0.5mmol phenylacetylene and 1mmol anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube mouth, and the reaction was stopped after magnetic stirring at 80°C for 5h, and the catalyst and supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 99%, and the selectivity of the target product diphenylacetylene was 95.1%.

[0074] Example 5

[0075] 20 mg of Pd 86 Cu 14 / CN double single atom catalyst and stirrer were placed in a reaction tube, 10mL ethanol, 0.5mmol iodobenzene, 0.5mmol phenylacetylene and 1mmol anhydrous potassium carbonate were added, N2 was introduced as protective gas and a balloon sealing system was connected to the condenser tube mouth, and the reaction was stopped after magnetic stirring at 80°C for 5h, and the catalyst and supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 99%, and the selectivity of the target product diphenylacetylene was 87.6%.

[0076] Example 6

[0077] 20 mg of Pd 37 Cu 63 / CN double single atom catalyst and stirrer were placed in a reaction tube, 10mL ethanol, 0.5mmol iodobenzene, 0.5mmol phenylacetylene and 1mmol anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube mouth. After magnetic stirring at 80°C for 5h, the reaction was stopped, and the catalyst and supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 49.8%, and the selectivity of the target product diphenylacetylene was 99.1%.

[0078] Comparative Example 5

[0079] 20 mg of Cu / CN single atom catalyst and a stirrer were placed in a reaction tube, 10 mL of ethanol, 0.5 mmol of iodobenzene, 0.5 mmol of phenylacetylene and 1 mmol of anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube mouth. After 5 hours of magnetic stirring at 80°C, the reaction was stopped, and the catalyst and the supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was <1.0%, and the target product diphenylacetylene was not detected.

[0080] Comparative Example 6

[0081] 20 mg of Pd / CN single atom catalyst and a stirrer were placed in a reaction tube, 10 mL of ethanol, 0.5 mmol of iodobenzene, 0.5 mmol of phenylacetylene and 1 mmol of anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube mouth. After 5 hours of magnetic stirring at 80°C, the reaction was stopped, and the catalyst and the supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 99%, and the selectivity of the target product diphenylacetylene was 82.9%.

[0082] Comparative Example 7

[0083] 10mg of Pd / CN and 10mg of Cu / CN two single-atom catalysts and a stirrer were placed in a reaction tube, 10mL of ethanol, 0.5mmol of iodobenzene, 0.5mmol of phenylacetylene and 1mmol of anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube mouth, and the reaction was stopped after 5h of magnetic stirring at 100°C, and the catalyst and supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 79.3%, and the selectivity of the target product diphenylacetylene was 99.3%. Compared with Example 4 (the atomic ratio of Pb and Cu was close to that of Comparative Example 7), the conversion rate of Comparative Example 7 was significantly lower.

[0084] Comparative Example 8

[0085] 10 mg of PdCu alloy nanocatalyst and a stirrer were placed in a reaction tube, 10 mL of ethanol, 0.5 mmol of iodobenzene, 0.5 mmol of phenylacetylene and 1 mmol of anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube port, and the reaction was stopped after magnetic stirring at 100 ° C for 5 hours, and the catalyst and supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 0.78%, and the target product diphenylacetylene was not detected.

[0086] Example 7

[0087] 20 mg of Pd 54 Cu 46 / CN double single atom catalyst and stirrer were placed in a reaction tube, 10mL DMF, 0.5mmol iodobenzene, 0.5mmol phenylacetylene and 1mmol anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube mouth, and the reaction was stopped after magnetic stirring at 80°C for 5h, and the catalyst and supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 21.5%, and the selectivity of the target product diphenylacetylene was 85.8%.

[0088] Example 8

[0089] 20 mg of Pd 54 Cu 46 / CN double single atom catalyst and stirrer were placed in a reaction tube, 10mL toluene, 0.5mmol iodobenzene, 0.5mmol phenylacetylene and 1mmol anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube mouth, and the reaction was stopped after magnetic stirring at 80°C for 5h, and the catalyst and supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 14.8%, and the selectivity of the target product diphenylacetylene was 55.1%.

[0090] Example 9

[0091] 20 mg of Pd 54 Cu 46 / CN double single atom catalyst and stirrer were placed in a reaction tube, 10mL DMF, 0.5mmol bromobenzene, 0.5mmol phenylacetylene and 1mmol anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube mouth, and the reaction was stopped after magnetic stirring at 140°C for 9h, and the catalyst and supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 75.3%, and the selectivity of the target product diphenylacetylene was 95.2%.

[0092] Example 10

[0093] 20 mg of Pd 54 Cu 46 / CN double single atom catalyst and stirrer were placed in a reaction tube, 10mL ethanol, 0.5mmol chlorobenzene, 0.5mmol phenylacetylene and 1mmol anhydrous potassium carbonate were added, N2 was introduced as a protective gas and a balloon sealing system was connected to the condenser tube mouth. After magnetic stirring at 140°C for 9h, the reaction was stopped, and the catalyst and supernatant were separated by centrifugation after cooling to room temperature. The standard curves of the target product diphenylacetylene and the reactant phenylacetylene were obtained by synchronous fluorescence detection, and the detection conversion rate was 39.6%, and the selectivity of the target product diphenylacetylene was 94.9%.

Claims

1. A bimetallic single-atom carbon-based catalyst, the carbon-based catalyst comprising a carbon-based carrier, the carrier carrying two metal single atoms of palladium and copper, the atomic ratio of palladium to copper is 0.9-1:0.9-1; the average distance between the palladium and copper atoms is 2.5 to 3.5 angstroms, and the carbon-based carrier is a carbon-nitrogen material.

2. According to the carbon-based catalyst according to claim 1, the ratio of the weight of the carbon-based carrier to the total weight of palladium and copper is 62500 ~ 45454: 1~2.

3. A method for preparing the carbon-based catalyst according to claim 1 or 2, comprising the following steps: a. Styrene, surfactant and thermal initiator are placed in deionized water, heated and stirred, cooled, and the resulting precipitate is dispersed in a polar solvent after centrifugal washing; b. Using the precipitate obtained in step a as a template, adding small molecular carbon nitrogen compounds and palladium and copper precursor salts to a buffer solution with a pH of 7-10, centrifuging, washing and drying to obtain a catalyst precursor; c. calcining the product obtained in step b at 700-900°C to obtain a powdered sample; d. The powdered sample obtained in step c is treated with acid, centrifuged, washed and dried to obtain a double single-atom catalyst.

4. The preparation method according to claim 3, wherein the surfactant in step a is selected from one or more of cetyltrimethylammonium bromide (CTAB), cetyltrimethylammonium chloride (CTAC), polyvinylpyrrolidone (PVP) and sodium dodecylbenzene sulfonate (SDBS).

5. The preparation method according to claim 3, wherein the thermal initiator described in step a is an inorganic peroxide initiator.

6. The preparation method according to claim 3, wherein the small molecule carbon-nitrogen compound in step b is selected from one or a combination of melamine, dicyandiamide, pyridine, urea and cyanoguanidine.

7. Use of the carbon-based catalyst according to claim 1 or 2 in catalyzing the coupling reaction of phenylacetylene and halogenated benzene, characterized in that: The amount of catalyst used in the reaction is 1%-3% of the mass of the reactants, the reaction temperature is 70-140° C., and the reaction time is 4-24 h.

8. The use according to claim 7, wherein the catalytic conversion rate of the reaction is above 98%, and the selectivity of the reaction is above 92%.

9. The use according to claim 8, wherein the halogenated benzene is selected from one or a combination of two or more of iodobenzene, chlorobenzene and bromobenzene.