A method for preparing atomic point defects and a structure having atomic point defects

By growing an amorphous structure film on the substrate and performing annealing treatment, the problem of complex atomic point defect preparation processes in the existing technology is solved, the process is simplified and the difficulty is reduced, and the use of a variety of substrate materials is supported.

CN115679300BInactive Publication Date: 2024-10-29INST OF ELECTRONICS ENG CHINA ACAD OF ENG PHYSICS
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202211397554.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-09
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The preparation process of atomic point defects in the existing technology is complicated and difficult. Especially when growing a crystal structure film on a sapphire substrate through MOCVD or MBE, the process control is complicated.

Method used

A thin film with an amorphous structure is grown on the substrate, and atomic point defects are formed through annealing, which simplifies the preparation process and reduces the difficulty. Specific steps include preparing the substrate, growing an island-like film with an amorphous structure, and activating atomic point defects in high-temperature annealing.

Benefits of technology

It simplifies the preparation process of atomic point defects, reduces the difficulty, and allows the use of a variety of substrate materials, including hard and flexible substrates, improving the controllability and flexibility of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115679300B_ABST
    Figure CN115679300B_ABST
Patent Text Reader

Abstract

The present application discloses a method for preparing the atomic point defects provided in the present application, including: preparing a substrate; growing a thin film of an amorphous structure on the upper surface of the substrate, wherein the thin film of the amorphous structure is in an island shape on the upper surface of the substrate; annealing the thin film of the amorphous structure to form atomic point defects in the thin film of the amorphous structure. In the present application, when preparing the atomic point defects, a thin film of an amorphous structure is grown on a prepared substrate. Since the thin film is of an amorphous structure, there is no need to consider the crystal growth quality of the thin film, and there are no atomic point defects in the thin film of the amorphous structure. By annealing the thin film of the amorphous structure, the atomic point defects in the thin film of the amorphous structure are activated, and atomic point defects are formed in the thin film of the amorphous structure, thereby obtaining atomic point defects. The preparation method of the present application has a simple process and low preparation difficulty. The present application also provides a structure with atomic point defects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of atomic point defect preparation, and in particular to a method for preparing an atomic point defect and a structure having an atomic point defect. Background Art

[0002] Atomic point defects have wide application potential in single photon sources, quantum bits and other applications. At present, when forming atomic point defects, MOCVD (Metal-organic Chemical Vapor Deposition) or MBE (Molecular Beam Epitaxy) is usually used to grow a crystalline film on a sapphire substrate or a homogeneous substrate. The crystalline film has atomic point defects. However, the process control of growing a crystalline film by MOCVD or MBE is complex and difficult, that is, the preparation process of atomic point defects is complex and difficult.

[0003] Therefore, how to solve the above technical problems should be the focus of technical personnel in this field. Summary of the invention

[0004] The purpose of the present application is to provide a method for preparing an atomic point defect and a structure having an atomic point defect, so as to simplify the preparation process of the atomic point defect and reduce the difficulty of preparation.

[0005] In order to solve the above technical problems, the present application provides a method for preparing atomic point defects, comprising:

[0006] preparing a substrate;

[0007] Growing a thin film with an amorphous structure on the upper surface of the substrate, wherein the thin film with an amorphous structure is in an island shape on the upper surface of the substrate;

[0008] The thin film with a non-crystalline structure is annealed to form atomic point defects in the thin film with a non-crystalline structure.

[0009] Optionally, growing a thin film with an amorphous structure on the upper surface of the substrate includes:

[0010] A thin film with an amorphous structure is grown on the upper surface of the substrate by using any one of atomic layer deposition technology, ion beam deposition technology and magnetron sputtering technology.

[0011] Optionally, when the thin film with the amorphous structure is annealed, the annealing temperature is greater than 500° C. and the annealing time is greater than 3 seconds.

[0012] Optionally, the thickness of the substrate is greater than 150 μm.

[0013] Optionally, the substrate is a flexible substrate.

[0014] Optionally, the substrate is a hard substrate.

[0015] Optionally, the hard substrate is a silicon substrate.

[0016] The present application also provides a structure with atomic point defects, and the structure with atomic point defects is obtained by using any of the above-mentioned methods for preparing atomic point defects.

[0017] The method for preparing atomic point defects provided in the present application includes: preparing a substrate; growing a thin film with an amorphous structure on the upper surface of the substrate, wherein the thin film with an amorphous structure is in an island shape on the upper surface of the substrate; and annealing the thin film with an amorphous structure to form atomic point defects in the thin film with an amorphous structure.

[0018] It can be seen that in the present application, when preparing atomic point defects, a thin film with an amorphous structure is grown on a prepared substrate. Since the thin film is of an amorphous structure, there is no need to consider the crystal growth quality of the thin film, and there are no atomic point defects in the amorphous structure thin film. The atomic point defects in the amorphous structure thin film are activated by annealing the amorphous structure thin film, and atomic point defects are formed in the amorphous structure thin film, thereby obtaining atomic point defects. The preparation method of the present application has a simple process and low preparation difficulty.

[0019] In addition, the present application also provides a structure with atomic point defects. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present application or the technical solutions of the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0021] Figure 1 A flow chart of a method for preparing an atomic point defect provided in an embodiment of the present application;

[0022] Figure 2 A top view of a structure with atomic point defects provided in an embodiment of the present application. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the present application, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0024] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0025] As described in the background technology section, currently, when forming atomic point defects, MOCVD or MBE is usually used to grow a crystalline film on a sapphire substrate or a homogeneous substrate, and the crystalline film has atomic point defects. However, the process control of growing a crystalline film by MOCVD or MBE is complex and difficult, that is, the preparation process of atomic point defects is complex and difficult.

[0026] In view of this, the present application provides a method for preparing atomic point defects, please refer to Figure 1 ,include:

[0027] Step S101: preparing a substrate.

[0028] It should be noted that the present application does not limit the type of substrate, as long as it can withstand the temperature during annealing.

[0029] As a specific implementation, the substrate may be a hard substrate, including but not limited to a sapphire substrate, a glass sheet, a GaN substrate, an AlGaN substrate, an AlN substrate, and a silicon substrate.

[0030] Preferably, the hard substrate is a silicon substrate, so that the structure with atomic point defects can be integrated with the chip through the silicon substrate. However, in the prior art, when preparing atomic point defects, the substrate used can only be a sapphire substrate or a substrate of the same material as the crystalline thin film material, and a silicon substrate cannot be used.

[0031] As another specific implementation, the substrate may be a flexible substrate, including but not limited to a polyimide (PI) substrate, a polyethylene terephthalate (PET) substrate, and a polyethylene naphthalate diformic acid glycolester (PEN) substrate.

[0032] It should also be noted that the thickness of the substrate is not limited in the present application, as long as the substrate can be ensured to be not easily damaged. For example, the thickness of the substrate is greater than 150 μm.

[0033] Step S102: growing a thin film with an amorphous structure on the upper surface of the substrate, wherein the thin film with an amorphous structure is in an island shape on the upper surface of the substrate.

[0034] It should be noted that the present application does not limit the growth method of the amorphous structure film, and the method can be selected at will. For example, any one of atomic layer deposition (ALD), ion beam deposition (IBD), and magnetron sputtering technology can be used to grow the amorphous structure film on the upper surface of the substrate.

[0035] The material of the thin film with a non-crystalline structure includes but is not limited to GaN, AlGaN, and AlN. The thickness of the thin film with a non-crystalline structure is less than 5 μm.

[0036] It should be pointed out that the amorphous structure film generated in this step does not have atomic point defects.

[0037] Step S103: performing annealing treatment on the thin film with a non-crystalline structure to form atomic point defects in the thin film with a non-crystalline structure.

[0038] Optionally, when the amorphous structure film is annealed, the annealing temperature is greater than 500° C. and the annealing time is greater than 3 seconds. The annealing temperature and time are adjusted according to the type and density of atomic point defects required, and the suppression of point defects that do not need to be activated.

[0039] In the present application, when preparing atomic point defects, a thin film with an amorphous structure is grown on a prepared substrate. Since the thin film is amorphous, there is no need to consider the crystal growth quality of the thin film, and there are no atomic point defects in the amorphous thin film. The atomic point defects in the amorphous thin film are activated and formed in the amorphous thin film by annealing the amorphous thin film, thereby obtaining atomic point defects. The preparation method of the present application has a simple process and low preparation difficulty.

[0040] On the basis of the above embodiment, in one embodiment of the present application, before growing a thin film with an amorphous structure on the upper surface of the substrate, the method further includes:

[0041] The substrate is cleaned to remove impurities and dirt on the surface of the substrate to enhance the bonding strength between the amorphous structure film and the substrate.

[0042] The preparation method of the atomic point defect in the present application is introduced below using a specific case.

[0043] Step 1, preparing a silicon substrate, wherein the thickness of the silicon substrate is 500 μm;

[0044] Step 2: growing an amorphous film with a thickness of 1 μm on the surface of the silicon substrate by magnetron sputtering, wherein the growth rate of the amorphous film is 20 nm / s;

[0045] Step 3: Testing the thin film with a non-crystalline structure obtained in step 2 by mapping micro-area PL spectrum test, and finding that there is no PL (photoluminescence) luminescence from atomic point defects;

[0046] Step 4, performing rapid thermal annealing on the amorphous structure film obtained in step 2, with an annealing temperature of 700° C. and an annealing time of 20 seconds;

[0047] Step 5: The thin film with the crystal structure after annealing was tested by mapping micro-area PL spectrum test, and the atomic point defect PL luminescence was found. For the 533nm excitation light, the luminescence wavelength was in the range of 600nm to 2um.

[0048] The present application also provides a structure with atomic point defects, and the structure with atomic point defects is obtained by using the preparation method of atomic point defects described in any of the above embodiments.

[0049] Please refer to Figure 2 The structure with atomic point defects includes a substrate 1, a non-crystalline film 2 located on the upper surface of the substrate 1, atomic point defects 3 in the non-crystalline film 2, and the non-crystalline film 2 is in an island shape on the upper surface of the substrate 1.

[0050] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0051] The above is a detailed introduction to the preparation method of atomic point defects and the structure with atomic point defects provided by the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.

Claims

1. A method for preparing atomic point defects, characterized in that: include: Preparing a substrate; the thickness of the substrate is greater than 150 μm; The substrate is a flexible substrate or the substrate is a hard substrate; A non-crystalline film is grown on the upper surface of the substrate, wherein the non-crystalline film is in an island shape on the upper surface of the substrate; the non-crystalline film has no atomic point defects; the growth rate of the non-crystalline film is 20 nm / s; the material of the non-crystalline film includes GaN, AlGaN, and AlN; the thickness of the non-crystalline film is less than 5 μm; Annealing the thin film with the amorphous structure to form atomic point defects in the thin film with the amorphous structure and activate the atomic point defects in the thin film with the amorphous structure; when annealing the thin film with the amorphous structure, the annealing temperature is 700° C. and the annealing time is 20 seconds; The step of growing a thin film with an amorphous structure on the upper surface of the substrate comprises: A thin film with an amorphous structure is grown on the upper surface of the substrate by using any one of atomic layer deposition technology, ion beam deposition technology and magnetron sputtering technology.

2. The method for preparing atomic point defects according to claim 1, characterized in that: The hard substrate is a silicon substrate.

3. A structure having atomic point defects, characterized in that: The structure having atomic point defects is obtained by using the method for preparing atomic point defects as described in any one of claims 1 to 2.

Citation Information

Patent Citations

  • AlN thin film grown on W substrate and preparation method and application of AlN thin film

    CN104143596A

  • II-VI based light emitting semiconductor device

    CN104428910A

  • Manufacturing method of silicon-based gallium nitride LED epitaxial structure

    CN105914270A

  • High-quality semi-polar indium gallium nitride two-dimensional ultrathin layer structure and preparation method thereof

    CN109830581A

  • Method for growing thin film on semiconductor substrate and application of method

    CN113224140A