Uniform warp-filled yarn
By selecting UHMWPE with high intrinsic viscosity and an appropriate amount of filler in the multifilament yarn, controlling the linear density and toughness change coefficient of the yarn, the breakage problem of the multifilament yarn during the manufacturing and processing process in the existing technology is solved, and the problem is achieved The result is more uniform yarn properties and higher tenacity, reducing production costs.
Patent Information
- Application Number
- CN202211346578.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-07-14
- Filing Date
- 2018-07-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2038-07-13
AI Technical Summary
Existing filled multifilament yarns have problems with filament breakage and yarn breakage during manufacturing and processing, resulting in reduced product quality, increased equipment downtime, and difficult processing.
By selecting UHMWPE with higher intrinsic viscosity and an appropriate amount of filler, the linear density and tenacity change coefficient of the yarn are controlled in a lower range, and the spinning process and stretching steps are used to form a uniform multifilament yarn to ensure that the yarn Stability during manufacturing and processing.
It achieves improvements in yarn uniformity and mechanical properties, avoids filament and yarn breakage, improves operability and production efficiency, and reduces costs while maintaining high yarn tenacity.
Smart Images

Figure BDA0003918515050000047 
Figure BDA0003918515050000111 
Figure BDA0003918515050000151
Abstract
Description
[0001] This application is a divisional application of Chinese patent application 201880045946.6 (PCT / EP2018 / 069139) with a filing date of July 13, 2018. Technical Field
[0002] The present invention relates to a filled multifilament yarn, comprising: a multifilament yarn having a certain intrinsic viscosity The invention relates to a UHMWPE having a diameter of at most 20 μm, a filler having a quantity of filler such that the ratio of the mass of filler to the total mass of UHMWPE and filler is between 0.02 and 0.50. In addition, the invention relates to a method for producing the filled multifilament yarn. The invention also relates to the use of the filled multifilament yarn in various applications. Background Art
[0003] Such filled multifilament yarns are known, for example, from documents WO2008046476 and WO2013149990. These documents disclose yarns with high cut resistance, which yarns comprise a hard component having a Mohs hardness of at least 2.5, the hard component being a plurality of hard fibers having an average diameter of at most 25 μm. However, the cut-resistant yarns disclosed in these documents show a high coefficient of variation, which makes processing difficult during the manufacture of the yarn and / or during further processing to obtain different products (e.g. knitting for the manufacture of gloves). This can lead to filament breakage and the generation of fuzz and ultimately to yarn breakage, resulting in reduced product quality and increased equipment downtime. Summary of the invention
[0004] The object of the present invention is therefore to provide a lengthy body which limits or even prevents filament or even yarn breakage during yarn manufacture and during processing of the yarn into articles, the filled multifilament yarn being producible at low cost and in an environmentally friendly manner while exhibiting high yarn tenacity.
[0005] This object is achieved by a filled multifilament yarn according to the invention, wherein at least (i) the coefficient of variation of the linear density between the filaments of the yarn is at most 12%, (ii) the coefficient of variation of the tenacity (ten) between the filaments of the yarn is at most 12%, or (iii) the coefficient of variation of the tenacity (TEN) of the multifilament yarn is at most 1.0%. The production of such filled multifilament yarn is achieved at less than 333 times the ratio of the filler mass to the total mass of UHMWPE and filler.
[0006] A method for producing a yarn with a reduced coefficient of variation, in particular a reduced coefficient of variation of the filament linear density (dpf), has been described in WO2009124762. WO2009124762 describes a gel spinning process in which a chamber is present before the spinneret so that no further distribution of the UHMWPE solution occurs before the final division of the UHMWPE solution into individual filaments, and at a constant throughput of the UHMWPE solution, the residence time of the solution in the chamber is at least 50 seconds. However, this method leads only to a limited improvement in the coefficient of variation and is not feasible for spinning UHMWPE solutions containing fillers.
[0007] The advantage of the yarn of the present invention is that the yarn is more uniform, that is, the individual filaments of the yarn show less difference from each other in mechanical and physical properties. The yarn of the present invention also has improved mechanical and physical properties. In addition, it is surprisingly found that the yarn of the present invention shows improved operability, particularly at an increased speed, such as in a coating process or in a process comprising yarn winding and / or high-speed yarn transportation. It is observed that in the process of yarn manufacturing and processing into articles, the filled multifilament yarn according to the present invention limits or prevents filament breakage and subsequent yarn breakage, which avoids quality problems and downtime during production. In addition, the filled multifilament yarn according to the present invention can be manufactured at low cost and can be produced with the same high yarn tenacity.
[0008] In the context of the present invention, a multifilament yarn or simply a yarn is understood to mean an elongated body comprising a plurality of, i.e. at least two, fibers. In this article, a fiber is understood to be an elongated body having a length dimension much greater than its transverse dimension (e.g. width and thickness). The term "fiber" includes monofilaments, ribbons, strips or bands, etc., and may have a regular or irregular cross-section. The fiber may have a continuous length, referred to in the art as a filament; or a discontinuous length, referred to in the art as a staple fiber.
[0009] The filled multifilament yarn of the present invention comprises a material having a certain intrinsic viscosity In the present context, UHMWPE is understood to be a polyethylene having an intrinsic viscosity (IV) of at least 5 dL / g, measured as a solution in decalin at 135°C. Preferably, the IV of the UHMWPE is at least 6 dL / g, more preferably at least 7 dL / g, most preferably at least 8 dL / g. Preferably, the IV is at most 20 dL / g, more preferably at most 18 dL / g, even more preferably at most 16 dL / g.
[0010] The filled multifilament yarn according to the invention preferably contains 2.0 to 50% by weight, preferably 4.0 to 40% by weight, preferably 5.0 to 35% by weight, even more preferably 6.0 to 30% by weight of filler, based on the total weight of filler and UHMWPE present in the fibers of the multifilament yarn. The amount of filler can alternatively be expressed as a filler ratio x, which is the ratio of the mass of filler to the total mass of UHMWPE and filler present in the fibers of the multifilament yarn. In line with the above, the ratio x is from 0.02 to 0.50, preferably from 0.04 to 0.40, also preferably from 0.05 to 0.35, even more preferably from 0.06 to 0.30.
[0011] An important aspect of the present invention is the discovery that when the levels of UHMWPE and filler are carefully selected during the manufacturing process, in particular the intrinsic viscosity of the UH used in the process should be at most 333 times the packing ratio (χ), in other words The uniformity of the filled multifilament yarn of UHMWPE can be improved. Preferably, the level of filler and UHMWPE should be such that Best More preferred Even more preferred Best choice It was observed that this relationship between the filler ratio and the IV of the UHMWPE used in the spinning process unexpectedly resulted in obtaining uniform multifilament yarns, thereby enabling the stable production of uniform multifilament yarns at higher filler levels than those described in the prior art. The lower limit of the relationship between the intrinsic viscosity of the UHMWPE used in the spinning process and the filler ratio is not particularly limited, but the content of filler and the IV of the UHMWPE are Should make Best
[0012] During the manufacture of the yarn of the invention, the UHMWPE undergoes a combination of thermal, mechanical and chemical degradation, resulting in a reduction in the intrinsic viscosity of the UHMWPE. Thus, the intrinsic viscosity of the UHMWPE present in the yarn of the invention is Different from and lower than the intrinsic viscosity of the UHMWPE supplied to the manufacturing process It has been experimentally determined that the reduction in IV during the manufacturing process is between 25% and 40%, but depends on a variety of parameters, such as polymer concentration, filler content, solvent type, processing temperature, etc. Therefore, in one embodiment of the present invention, the multifilament yarn comprises a certain intrinsic viscosity. The intrinsic viscosity of UHMWPE is at most 225 times the filler ratio (χ) as defined above, in other words, Preferably, the level of filler and the IV of the UHMWPE should be such that Best More preferred Best choice
[0013] In one embodiment of the present invention, the uniformity of a multifilament yarn is expressed as the coefficient of variation of the linear density (dpf) between the (single) filaments of the yarn (hereinafter referred to as ) is at most 12%, of which the yarn is determined by linear density values x corresponding to 10 representative lengths, each of which corresponds to a different randomly sampled filament of said yarn, and using Formula 1,
[0014]
[0015] where x i is the linear density at any of the 10 representative lengths studied, and is the average linear density over the n=10 measured linear densities of said n=10 representative lengths. Less than 10%, more preferably less than 8%. A filled multifilament yarn of high value is obtained, for example, by the process of the invention as described below.
[0016] In an alternative embodiment of the present invention, the uniformity of a multifilament yarn is expressed as the coefficient of variation of the tenacity (ten) between the (single) filaments of the yarn (hereinafter referred to as ) is at most 12%, of which the yarn determined by the tenacity values y corresponding to 10 representative lengths, each of which corresponds to a different randomly sampled filament of said yarn, using Formula 2,
[0017]
[0018] where y i is the toughness at any of the 10 representative lengths studied, and is the average tenacity over the n=10 measured tenacities at said n=10 representative lengths. Less than 10%, more preferably less than 8%. A filled multifilament yarn of high value is obtained, for example, by the process of the invention as described below.
[0019] In a third alternative preferred embodiment of the present invention, the uniformity of the multifilament yarn is expressed as follows: ) is at most 1.0%, wherein Determined by the yarn tenacity values z corresponding to 5 representative yarn lengths randomly sampled from the multifilament yarn and using Formula 3,
[0020]
[0021] where z i is the yarn tenacity for any of the five representative yarn lengths studied, and is the average yarn tenacity over the n=5 measured tenacities of said n=5 representative yarn lengths. Less than 0.8%, more preferably less than 0.6%. A filled multifilament yarn having a value of is obtained, for example, by the process of the invention as described below. This embodiment of the invention is obtained by the commonly reported The value is used to demonstrate the commercial significance of the invention and to prove the consistency of the production process.
[0022] In the above embodiments, the representative yarn length and the representative filament length of a single filament are to be understood as the length of the yarn or filament from the same production period, i.e. a sample of several hundred meters during or after the production process, rather than the length spread over the entire (commercial) production run. Thus, the representative filament length of the yarn is a sample selected randomly from a specific portion of the yarn rather than from different yarn portions, let alone from different yarn portions spread over the production process.
[0023] In the context of the present invention, fillers are understood to be components that are immiscible with UHMWPE and are substantially solid under the processing conditions of UHMWPE multifilament yarns. Such fillers can affect one or more properties of the yarn, such as its density, cut resistance, color, wear resistance, etc. The filler may include particles made of a material having a hardness greater than the hardness of the molded article measured without the filler or composed of the particles, and may be organic or inorganic. If the filler is organic, it is preferably a polymer having a melting temperature of at least 150°C, preferably at least 200°C. Preferably, the material is an inorganic material. In the context of the present invention, inorganic materials are understood to be materials that are substantially free of covalently bonded carbon atoms, and therefore do not include any organic materials, such as hydrocarbons, especially polymeric materials. In particular, inorganic materials refer to compounds including metals, metal oxides, clays, silica, silicates or mixtures thereof, but also include carbides, carbonates, cyanides and allotropes of carbon, such as diamonds, graphite, graphene, fullerenes and carbon nanotubes. The use of fillers comprising inorganic materials provides the multifilament yarn with optimized secondary properties, such as abrasion resistance and cut resistance.Preferably, the inorganic material is glass fiber, mineral fiber, metal fiber or carbon fiber.
[0024] Preferably, the material used to produce the filler has a Mohs hardness of at least 2.5, more preferably at least 4, and most preferably at least 6. Useful materials include, but are not limited to, metals, metal oxides (e.g., aluminum oxide), metal carbides (e.g., tungsten carbide), metal nitrides, metal sulfides, metal silicates, metal silicides, metal sulfates, metal phosphates, and metal borides. Other examples include silicon dioxide and silicon carbide. Other ceramic materials and combinations of the above materials may also be used.
[0025] The particle size, particle size distribution, particle diameter and dosage of the filler are all important parameters for optimizing yarn properties (such as cut resistance) while obtaining a uniform multifilament yarn. Fillers can be used in particulate form, and powders are generally suitable. For particles that have no other size that is significantly larger than the particle, such as spherical or cubic particles, the average particle size is essentially equal to the average particle diameter, or simply the diameter. In the context of the present invention, if not otherwise specified, the average value is an exponential average. For substantially elliptical particles, such as elongated or non-spherical or anisotropic materials (such as needles, fibrils or fibers), the particle size may refer to the average length dimension (L) along the long axis of the particle, while the average particle diameter, or also referred to herein as the diameter, refers to the average diameter of the cross section perpendicular to the length direction of the elliptical shape. In the case where the cross-section of the particle is not circular, the average diameter (D) is determined by the following formula: D=1.15*A 1 / 2 , where A is the cross-sectional area of the particle.
[0026] The selection of suitable particle size, diameter and / or length depends on the process and the filament fineness of the multifilament yarn. However, the particles should be small enough to pass through the spinneret holes. Small enough particle size and diameter can be selected to avoid a significant decrease in fiber tensile properties. Particle size and diameter can have a log-normal distribution.
[0027] The average diameter of the filler is at most 20 μm, preferably at most 15 μm, even more preferably at most 12 μm. Fillers with lower average diameters can lead to increased uniformity of the yarn and can lead to fewer surface defects on the filaments. Larger filler diameters lead to processing difficulties and deterioration of mechanical strength.
[0028] Preferably, the diameter of the filler is at least 0.01 μm, preferably at least 0.1 μm, even more preferably 1 μm, most preferably at least 3 μm. Fillers with a larger average diameter may lead to an optimized shaping step in the process of the invention.
[0029] Preferably, the average diameter of the filler is at least 0.01 μm and at most 20 μm, more preferably, the average diameter of the filler is at least 0.1 μm and at most 20 μm, even more preferably, the average diameter of the filler is at least 1 μm and at most 20 μm, most preferably, the average diameter of the filler is at least 3 μm and at most 20 μm, even most preferably, the average diameter of the filler is at least 3 μm and at most 16 μm, even most preferably, the average diameter of the filler is at least 3 μm and at most 12 μm.
[0030] Preferably, the average length (L) of the filler is at most 10000 μm, more preferably at most 5000 μm, most preferably at most 3000 μm. It has also been observed that the articles of the invention, in particular gloves comprising the filled multifilament yarn of the invention, show good dexterity when the average length of the filler is at most 1000 μm, more preferably at most 750 μm, most preferably at most 650 μm. Preferably, the average length of the hard fibers is at least 50 μm, more preferably at least 100 μm, most preferably at least 150 μm, even more preferably at least 200 μm.
[0031] The filler present in the filled multifilament yarn may be particles having an aspect ratio L / D of about 1. The filler present in the filled multifilament yarn may be in the form of fibers having an aspect ratio L / D of at least 3, preferably at least 5, even more preferably at least 10, more preferably at least 20. The filler in the multifilament yarn may comprise or consist of particles and / or fibers.
[0032] Any filler known in the art can be used. Suitable fillers are already commercially available, such as those used in the Examples section of the present invention. Fillers added to HPPE fibers and methods of adding fillers to HPPE fibers are well known to those skilled in the art, for example, described in documents WO9918156A1 (which is incorporated herein by reference), WO2008046476 (which is incorporated herein by reference), and WO2013149990 (which is incorporated herein by reference).
[0033] The aspect ratio of the filler is the ratio of the length, i.e., the average length (L), of the filler to the diameter, i.e., the average diameter (D). The average diameter and aspect ratio of the filler can be determined by using any method known in the art, such as SEM photos. In order to measure the diameter, a SEM image of the filler can be taken, for example, the fiber is spread on the surface as it is, and the diameter is measured at 100 randomly selected positions, and then the arithmetic mean of the 100 values obtained is calculated. For the aspect ratio, a SEM image of a filler (e.g., a fiber) can be taken, and the length of the filler (e.g., a fiber) can be measured, such as a fiber that appears on or below the surface of the HPPE fiber. The SEM image is preferably made with backscattered electrons to provide better contrast between the fiber and the HPPE fiber surface.
[0034] Filler can be continuous or spun fiber, particularly spun fiber. Suitable examples of spun fiber are glass or mineral fibers, which can be spun by rotary techniques well known to technicians. Fiber can be made into continuous filaments, which are subsequently ground into fibers of much shorter length. The grinding process can reduce the aspect ratio of at least a portion of the fiber. Alternatively, discontinuous filaments can be produced, for example, by jet spinning, optionally subsequently ground and used for multifilament yarn of the present invention. In the production process of multifilament yarn, fiber may be subjected to a reduction in aspect ratio.
[0035] Carbon fibers may be used as fillers. Most preferably, carbon fibers having a diameter between 3 and 10 μm, more preferably between 4 and 6 μm, are used. Articles comprising carbon fibers show improved electrical conductivity and are able to discharge static electricity.
[0036] The filaments in the filled multifilament yarn, also called monofilaments, may have a linear density of up to 20 dtex, preferably up to 15 dtex, most preferably up to 10 dtex, because articles containing such filaments are very soft, thereby providing a high level of comfort to the person wearing the article. The titer of the filaments is preferably at least 1 dtex, more preferably at least 2 dtex.
[0037] The titer of the filled multifilament yarn is not particularly limited. For practical reasons, the titer of the multifilament yarn may be at most 10000 dtex, preferably at most 6000 dtex, more preferably at most 3000 dtex. Preferably, the titer of the yarn is in the range of 50 to 10000 dtex, more preferably in the range of 100 to 6000 dtex, and most preferably in the range of 200 to 3000 dtex, still more preferably in the range of 220 to 800 dtex, still more preferably 100 to 2000 dtex.
[0038] The filled multifilament yarn of the present invention is preferably a high performance polyethylene (HPPE) yarn, and preferably the tenacity of the multifilament yarn is at least 5.0 cN / dtex, more preferably at least 7.5 cN / dtex, even more preferably at least 10.0 cN / dtex, more preferably at least 12.5 cN / dtex, even more preferably at least 15.0 cN / dtex, and most preferably at least 20.0 cN / dtex.
[0039] The yarn according to the invention shows an improvement in strength efficiency, making it possible to achieve higher filler contents, thus providing the filled multifilament yarn with further improved cut resistance. The strength (or tenacity) efficiency is understood herein as the strength (tenacity, TEN) in cN / dtex obtained by the multifilament yarn divided by the intrinsic viscosity of the UHMWPE present in said yarn. Other forms of ratios For unfilled yarns, this efficiency is typically in the range of 0.5 to 1.5, with a higher efficiency being an indicator of a more optimized production process. The presence of fillers during the production process can significantly affect (i.e., reduce) the strength efficiency. In contrast, the yarns of the present invention exhibit an improved strength efficiency. Preferably, the yarns according to the present invention have a strength efficiency such that the strength (tenacity) obtained at varying filler contents complies with Or rewritten as Preferably, the tenacity of the filled multifilament yarn is such that More preferred And the best choice
[0040] In the context of the present invention, UHMWPE can be linear or branched, wherein linear polyethylene is preferred. Linear polyethylene is understood herein to mean polyethylene having less than 1 side chain per 100 carbon atoms, preferably less than 1 side chain per 300 carbon atoms, wherein the side chain or branching generally contains at least 10 carbon atoms. The side chain can be appropriately measured by FTIR. Linear polyethylene may further comprise up to 5 mol% of one or more other olefins copolymerizable therewith, such as propylene, 1-butene, 1-pentene, 4-methylpentene, 1-hexene and / or 1-octene.
[0041] The filled multifilament yarn of the present invention leads to an improved manufacturing process and higher quality articles made from the yarn. Therefore, one embodiment of the present invention relates to an article comprising the filled multifilament yarn of the present invention. The article containing the yarn of the present invention can be, but is not limited to, a product selected from the group consisting of: fishing lines, fish nets, ground nets, cargo nets, curtains, kite lines, dental floss, tennis racket lines, canvas, woven fabrics, nonwoven fabrics, webbing, battery separators, medical devices, capacitors, pressure vessels, hoses, umbilical cables, automotive equipment, power transmission belts, building materials, cut-resistant articles, puncture-resistant articles, incision-resistant articles, protective gloves, composite sports equipment, skis, helmets, kayaks, canoes, bicycles and boat hulls, speaker cones, high performance electrical insulation, radomes, sails and geotextiles.
[0042] Fabrics comprising the filled multifilament yarn according to the invention can be produced by knitting, weaving or by other methods using conventional equipment. Nonwoven fabrics can also be produced. The cut resistance of the fabric comprising the yarn according to the invention can be 20% higher than the same fabric produced from yarn without filler, the cut resistance being measured according to the Ashland Cut Protection Performance Test. Preferably, the cut resistance of the fabric is increased by at least 50%, more preferably by at least 100%, even more preferably by at least 150%.
[0043] The filled multifilament yarn according to the invention is suitable for use in all kinds of products, for example in clothing for protecting people working in the meat industry, metal industry and wood industry from cuts. Good examples of such clothing include gloves, aprons, pants, cuffs, sleeves, etc. Other possible applications include side curtains and tarpaulins for trucks, soft luggage, commercial decoration, air container curtains, fire hose protective covers, etc. Surprisingly, the yarn according to the invention is very suitable for use in stab-proof products, for example in products for protection against knife stabs or ice pick stabs. An example of such a product is a life-saving protective vest for police officers.
[0044] Preferably, in such structures, the yarn of the present invention is located on the side of the structure that is likely to be struck first by a sharp object used in an attack.
[0045] The filled multifilament yarn can be obtained by various methods known in the art, for example, by a melt spinning process or a gel spinning process as described herein. The gel spinning process is described in various publications such as EP0205960 A, EP 0213208 A1, US 4413110, GB 2042414 A, EP 0200547 B1, EP 0472114 B1, WO 01 / 73173 A1 and Advanced Fiber Spinning Technology, Ed. T. Nakajima, Woodhead Publ. Ltd (1994), ISBN1-855-73182-7 and references cited therein. Gel spinning is understood to include at least the following steps: spinning multifilaments from a solution of ultra-high molecular weight polyethylene in a spinning solvent; cooling the resulting filaments to form gel filaments; removing at least part of the spinning solvent from the gel filaments; and stretching the filaments in at least one stretching step before, during or after the removal of the spinning solvent.
[0046] In the process according to the invention, any known solvent suitable for gel spinning of UHMWPE may be used, hereinafter such solvent being referred to as spinning solvent. Suitable examples of spinning solvents include aliphatic and alicyclic hydrocarbons, such as octane, nonane, decane and paraffin, including their isomers; petroleum fractions; mineral oils; kerosene; aromatic hydrocarbons, such as toluene, xylene and naphthalene, including their hydrogenated derivatives, such as decalin and tetralin; halogenated hydrocarbons, such as monochlorobenzene; and cycloalkanes or cycloalkenes, such as carene, fluorene, camphene, menthane, dipentene, naphthalene, acenaphtalene, methylcyclopentadiene, tricyclodecane, 1,2,4,5-tetramethyl-1,4-cyclohexadiene, fluorenone, naphtindane, tetramethylbenzene, ethylfluorene, fluoranthene and naphthenone. Gel spinning of UHMWPE can also be carried out using combinations of the spinning solvents listed above, which for simplicity are also referred to as spinning solvents. We have found that the process of the present invention is particularly advantageous for relatively volatile solvents such as decalin, tetralin and several kerosene fractions. In a most preferred embodiment, the solvent of choice is decalin. The spinning solvent can be removed by evaporation, extraction or a combination of evaporation and extraction routes.
[0047] The invention also relates to a method for preparing a filled multifilament yarn according to the invention, comprising the following steps:
[0048] a) Provide intrinsic viscosity less than 24 dL / g, preferably less than 20 dL / g of UHMWPE,
[0049] b) providing a filler having an average diameter of at most 20 μm,
[0050] c) preparing a solution of the UHMWPE in a solvent, the solution comprising the filler in an amount such that the ratio (χ) of the mass of the filler to the total mass of the UHMWPE and the filler is between 0.02 and 0.50,
[0051] d) spinning the solution obtained in step c) through a porous die plate to form a filled multifilament yarn comprising a solvent,
[0052] e) at least partially removing the solvent from the warp-stuffed yarn of step d) before, during or after drawing the stuffed yarn at an overall draw ratio of at least 20,
[0053] To obtain the filled multifilament yarn, wherein the provided UHMWPE is selected such that
[0054] The selection of UHMWPE, filler and ratio χ is preferably carried out according to the previously preferred embodiments for said UHMWPE, filler and ratios for defining the embodiments of the filled multifilament yarn of the present invention. Therefore, a preferred embodiment of the method of the present invention is to select the ratio of the mass of filler to the total mass of UHMWPE and filler (χ) to be 0.05 to 0.40, or other ranges and levels mentioned above. Another preferred embodiment of the method of the present invention is to select the filler ratio χ and UHMWPE such that Or within the preferred definitions provided above.
[0055] Standard equipment can be used for this process, preferably a twin-screw extruder is used, wherein in a first section the polymer is dissolved in a solvent, wherein at the end of the first section the fibers are fed to the extruder through a separate feed opening.
[0056] It is also possible to convert the yarn obtained by the above method into staple fibers and then process these staple fibers into yarn.
[0057] The scope of the invention also includes so-called composite yarns and products containing such yarns, which for example contain one or more single yarns containing filaments and / or staple fibers containing fillers and one or more additional single yarns or yarns, wires or filaments of glass, metal or ceramic.
[0058] In the method for preparing the filled multifilament yarn, the stretching, preferably uniaxial stretching, of the prepared yarn can be carried out by methods known in the art. Such methods include: extrusion stretching and tensile stretching on a suitable stretching unit. In order to obtain increased mechanical tensile strength and stiffness, the stretching can be carried out in multiple steps. The first stretching step, for example, includes stretching to an elongation factor (also referred to as a stretching factor) of at least 1.5, preferably at least 3.0. Multi-step stretching generally results in: for a stretching temperature of up to 120°C, an elongation factor of 9, for a stretching temperature of up to 140°C, an elongation factor of 25, and for a stretching temperature of up to and above 150°C, an elongation factor of 50. An elongation factor of about 50 or more may be achieved by multi-step stretching at elevated temperatures. This results in the possibility of obtaining a filled multifilament yarn with a tenacity of 5.0 cN / dtex to 30 cN / dtex and higher. Among them, for ultra-high molecular weight polyethylene tapes, strengths of 1.5 GPa to 1.8 GPa and higher can be obtained. The individual stretch ratios in the liquid phase, gel phase, and solid phase can be combined to express a total stretch ratio.
[0059] The filled multifilament yarn according to the present invention may further comprise other fibers, which may be in the form of filaments and / or staple fibers, which are different from the filled filaments, for example, in composition and / or shape, such as non-polymeric fibers, such as glass fibers, carbon fibers, basalt fibers, metal wires or threads; and / or natural fibers, such as cotton, bamboo; and / or polymer fibers, such as polyamide fibers (e.g. nylon fibers), elastic fibers (e.g. spandex), polyester fibers; and / or mixtures of these other fibers, which may be present in any proportions. DETAILED DESCRIPTION
[0060] The invention will be further explained by the following examples and comparative experiments, but first the methods used to determine the various parameters that can be used to define the present invention are described below.
[0061] method
[0062] Yarn linear density: The yarn titer is measured by weighing 100 meters of yarn. The weight (expressed in milligrams) is divided by 10 to give the yarn's dtex.
[0063] IV: The intrinsic viscosity of UHMWPE was determined according to the method ASTM-D1601 / 2004. The test conditions were: at 135°C, in decalin, the dissolution time was 16 hours, 2 g / l of DBPC was used as an antioxidant, and the viscosity measured at different concentrations was extrapolated to obtain the viscosity at zero concentration.
[0064] Tensile properties of yarns: Tenacity and modulus are defined and measured on multifilament yarns as specified in ASTM D885M using a nominal fiber length of 500 mm, a crosshead speed of 50% / min, and an Instron 2714 grip (Fibre Grip D5618C). The modulus is determined as the gradient between 0.3% and 1% strain from the measured stress-strain curve. To calculate modulus and strength, the measured tensile force is divided by the denier.
[0065] Tensile properties of filaments: According to the procedure of ISO 5079:1995, using a fiber with a nominal length of 50 mm, a crosshead speed of 25 mm / min and a The tenacity is defined and measured on the single filaments using a pneumatic gripper made of a 300-mm-diameter pneumatic gripper with a standard jaw surface (4*4 mm) using Textechno's Favimat (tester No. 37074, purchased from Textechno Herbert Stein GmbH & Co. KG, Monchengladbach, Germany). The filaments are preloaded with 0.04 cN / dtex at a speed of 25 mm / min. To calculate the tenacity, the measured tensile force is divided by the linear density (fineness) of the filament;
[0066] Linear density: The linear density of the monofilament was measured according to ASTM D1577-01 on a semi-automatic microprocessor-controlled tensile tester (Favimat, tester No. 37074, purchased from Textechno Herbert Stein GmbH & Co. KG, Monchengladbach, Germany). A representative length of the monofilament was cut from the monofilament with a sharp blade and sandwiched between two small pieces of paper (4×4 mm). The length is sufficient to ensure a good installation of the monofilament, approximately 70 mm.
[0067] As described above, the linear density of the length of monofilament between the jaws was determined by a vibrometer by following the routine implemented in the tester software and described in the tester manual. During the measurement, the distance between the jaws was kept at 50 mm and the monofilament was tensioned at 0.6 cN / dtex at a speed of 2 mm / min.
[0068] The number of olefinic branches per thousand carbon atoms was determined by FTIR on 2 mm thick pressed films, using a calibration curve based on NMR measurements to quantify the peak at 1375 cm -1 The amount of absorption at , as described, for example, in EP 0 269 151, in particular page 4.
[0069] • The average length and average diameter were measured by using the CottonscopeHD analysis system.
[0070] The amount of filler in the yarn (% by weight) was determined as the weight difference between the initial weight of the yarn and the weight of the yarn remaining after burning the polymer in the yarn (measured by weighing the ash content obtained after combustion). The combustion was performed by heating the yarn at a temperature of 700°C.
[0071] The cut resistance was determined according to ISO 13997-1999 after weaving a fabric with 260 g / m2 of the corresponding yarn.
[0072] Example
[0073] Comparative Experiment 1 (CE1)
[0074] The yarn is produced according to the method of Example 1 of WO2013149990: The UHMwPE of 27.0dL / g is dry mixed with 7% by weight of mineral fibrils (number average diameter of 7.4μm, average length of 70μm, Mohs hardness of 3.5) sold by Lapinus, NL under the trade name CF10ELS, and then dissolved in decalin to make the total solid content (i.e. the total content of polymer and filler) 9% by weight. The solution thus obtained is fed into a twin screw extruder with a screw diameter of 25mm equipped with a gear pump. In this way, the solution is heated to a temperature of 180°C. The solution is pumped through a spinneret with 64 holes, each of which has a diameter of 1 mm. The filaments thus obtained are stretched by a factor of 206 in total and dried in a hot air oven. After drying, the filaments are bundled into yarns and wound around a bobbin.
[0075] Comparative Experiment 2 (CE2)
[0076] Yarn was obtained as described for CE1, except that The UHMWPE of 22.0 dL / g and the mineral filler were used at a ratio of 6 wt%, and the obtained filaments were stretched by a factor of 207 in total.
[0077] Comparative Experiment 3 (CE3)
[0078] Another yarn was obtained as described for CE2, with the difference that the mineral filler was used at a rate of 15% by weight and the filaments obtained were stretched by a factor of 202 in total.
[0079] The tensile measurements reported in Table 1 were performed on the yarns of CE1, CE2 and CE3.
[0080] Yarns of CE2 (440 dtex) and CE3 (220 dtex) were woven into fabrics of 380 and 260 g / m2, respectively. The cut resistance of the fabrics was tested. The required cutting force (CF) was measured. The results are given in Table 1.
[0081] Example A (Ex A)
[0082] Yarn was obtained as described for yarn of CE2, except that UHMWPE with an IV of 17.0 dL / g was used and the obtained filaments were stretched by a factor of 204 in total.
[0083] Example B (Ex B)
[0084] Yarns were obtained as described for yarns of CE3, except that UHMWPE with an IV of 17.0 dL / g was used and the filaments obtained were stretched by a factor of 210 in total.
[0085] Table 1
[0086]
Claims
1. A filled multifilament yarn comprising: -Has a certain intrinsic viscosity UHMWPE, - a filler having a diameter of at least 1 μm and at most 20 μm and an aspect ratio of at least 3, in an amount such that the ratio χ of the mass of the filler to the total mass of UHMWPE and filler is between 0.02 and 0.50, -in - the coefficient of variation of the linear density dpf between the filaments of the yarn, hereinafter referred to as is at most 12%, of which the yarn is determined by linear density values x corresponding to 10 representative lengths, each of which corresponds to a different randomly sampled filament of said yarn, and using Formula 1, where x i is the linear density at any of the 10 representative lengths studied, and is the average linear density over the n=10 measured linear densities at said n=10 representative lengths.
2. A filled multifilament yarn comprising: -Has a certain intrinsic viscosity UHMWPE, - a filler having a diameter of at least 1 μm and at most 10 μm and an aspect ratio of at least 3, in an amount such that the ratio χ of the mass of the filler to the total mass of UHMWPE and filler is between 0.02 and 0.50, -in - wherein the coefficient of variation of the tenacity ten between the filaments of the yarn is hereinafter referred to as is at most 12%, of which the yarn determined by the tenacity values y corresponding to 10 representative lengths, each of which corresponds to a different randomly sampled filament of said yarn, using Formula 2, where y i is the linear density at any of the 10 representative lengths studied, and is the average linear density over the n=10 measured linear densities at said n=10 representative lengths.
3. The filled multifilament yarn according to any one of claims 1 to 2, in, The individual coefficients of variation were at most 10%.
4. A filled multifilament yarn comprising: -Has a certain intrinsic viscosity UHMWPE, - a filler having a diameter of at least 1 μm and at most 20 μm and an aspect ratio of at least 3, in an amount such that the ratio χ of the mass of the filler to the total mass of UHMWPE and filler is between 0.02 and 0.50, -in - wherein the coefficient of variation of the tenacity TEN of the multifilament yarn is hereinafter referred to as is at most 1.0%, wherein the multifilament yarn Determined by the tenacity values z corresponding to 5 representative yarn lengths randomly sampled from the multifilament yarn and using Formula 3, where z i is the tenacity of any of the five representative yarn lengths studied, and is the average tenacity over the n=5 measured tenacities of said n=5 representative yarn lengths.
5. The filled multifilament yarn according to claim 4, in, The coefficient of variation is at most 0.8%.
6. The filled multifilament yarn according to any one of claims 1, 2 or 4, in, The ratio χ of the filler mass to the total mass of UHMWPE and filler is between 0.05 and 0.
40.
7. The filled multifilament yarn according to any one of claims 1, 2 or 4, in, The yarn has a tenacity of at least 5.0 cN / dtex.
8. The filled multifilament yarn according to any one of claims 1, 2 or 4, in, The tenacity TEN of the yarn is 9. A method for preparing a filled multifilament yarn, The following steps are involved: a) Provide intrinsic viscosity Less than 20dL / g UHMWPE, b) providing a filler having an average diameter of at least 1 μm and at most 20 μm and an aspect ratio of at least 3, c) preparing a solution of the UHMWPE in a solvent, the solution comprising the filler in an amount such that the ratio x of the mass of the filler to the total mass of the UHMWPE and the filler is between 0.02 and 0.50, d) spinning the solution obtained in step c) through a porous template to form a filled multifilament yarn comprising a solvent, e) at least partially removing the solvent from the warp-stuffed yarn of step d) before, during or after drawing the stuffed yarn at an overall draw ratio of at least 20, to obtain said filled multifilament yarn, The UHMWPE provided is selected so that 10. The method according to claim 9, in, The ratio of the filler mass to the total mass of UHMWPE and filler, χ, is between 0.04 and 0.
40.
11. The method according to claim 9, in, 12. An article comprising the filled multifilament yarn of any one of claims 1 to 8.
13. The article according to claim 12, in, The article is selected from the group consisting of cut-resistant articles and stab-resistant articles.
14. The article according to claim 12, in, The article is selected from the group consisting of fishing lines, fish nets, ground nets, cargo nets, kite strings, dental floss, tennis racket strings, woven fabrics, nonwoven fabrics, battery separators, medical devices, capacitors, pressure vessels, hoses, umbilical cables, automotive equipment, power transmission belts, building materials, protective gloves, composite sports equipment, helmets, speaker cones, radomes, sails and geotextiles.