A method for preparing an adsorption dehumidification material for a dehumidification wheel

By using a composite slurry composed of sodium polyacrylate and water-based polyurethane to form a hygroscopic layer in the dehumidification wheel, the problems of high desorption temperature and insufficient mechanical strength in the existing technology are solved, and the effects of efficient dehumidification and low-temperature regeneration adsorption are achieved.

CN115679704BActive Publication Date: 2024-10-01JIANGSU SUJING GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211443675.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-26
Publication Date
2024-10-01
Estimated Expiration
2040-12-26

AI Technical Summary

Technical Problem

The desorption temperature of the core material of the existing dehumidification wheel is relatively high, making it difficult to balance high dehumidification capacity and low regeneration temperature. At the same time, it lacks good mechanical strength.

Method used

A composite slurry composed of sodium polyacrylate, water-based polyurethane and solvent is coated on the substrate to form a hygroscopic layer. Water-based polyurethane is generated through the reaction of polyisocyanate, hydrophilic polyol and hydroxyl-containing small molecule chain extender, combined with physical coagulation. Mixing technology is used to prepare adsorption and dehumidification materials for dehumidification rotors with excellent hygroscopic properties.

Benefits of technology

An adsorption dehumidification material with both high-efficiency dehumidification and strength at lower temperatures has been achieved, significantly reducing the regeneration energy consumption of the runner and improving the mechanical strength of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003949020360000061
    Figure BDA0003949020360000061
Patent Text Reader

Abstract

The invention discloses a preparation method of an adsorption dehumidification material for a dehumidification wheel. The preparation method comprises: making polyisocyanate and hydrophilic polyol undergo a first reaction to prepare a polyurethane prepolymer, adding a hydrophilic chain extender and a hydroxyl-containing small molecule chain extender with a molecular weight less than or equal to 200, carrying out a second reaction, adding a hydroxyl-containing water-soluble polymer, carrying out a third reaction to generate an aqueous polyurethane, dispersing the aqueous polyurethane in water for emulsification to prepare an aqueous polyurethane emulsion; dispersing sodium polyacrylate in water to prepare a sodium polyacrylate solution; mixing the sodium polyacrylate solution with the aqueous polyurethane emulsion to obtain a composite slurry; soaking a substrate in the composite slurry, and then drying to prepare the adsorption dehumidification material for a dehumidification wheel; the adsorption dehumidification material can be used as a wheel core material of a dehumidification wheel, especially can have both a high dehumidification capacity and a low regeneration temperature, and has properties such as good mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention is a divisional application of the Chinese invention patent application with application date of December 26, 2020, application number 2020115682437, and name “A kind of adsorption dehumidification material for dehumidification wheel, preparation method and application thereof”. Technical Field

[0002] The invention relates to the technical field of gas dehumidification, and in particular to a method for preparing an adsorption dehumidification material for a dehumidification wheel. Background Art

[0003] With the continuous improvement of people's living standards and the rapid development of production technology, the requirements for air humidity in various fields are getting higher and higher. Adding dehumidification equipment to the air conditioning system can significantly reduce the energy consumption of the air conditioning itself; in the food industry, air humidity control can effectively inhibit the growth of bacteria and extend the shelf life of products; in the semiconductor and electronics industry, there are strict requirements for the humidity conditions in the production workshop, and too high humidity will seriously affect product performance.

[0004] Traditional dehumidification technologies include refrigeration dehumidification, liquid absorbent dehumidification and solid adsorbent dehumidification. In addition, rotary dehumidification is also a commonly used dehumidification technology in industry. Compared with refrigeration dehumidification, rotary dehumidification can achieve a lower dew point; compared with liquid absorbent dehumidification, rotary dehumidification also avoids the corrosion problem of the desiccant; compared with solid adsorbent dehumidification, rotary dehumidification is continuous and the regeneration process is more convenient and simple. At present, the most commonly used wheel core materials in dehumidification wheels are silica gel and molecular sieves. Silica gel has a higher adsorption capacity, while molecular sieves are suitable for working conditions with low dew point requirements. However, even for silica gel wheels with lower desorption requirements, a desorption temperature of about 100°C is required. Therefore, how to reduce the desorption temperature as much as possible while meeting the dehumidification requirements has become a research hotspot for this type of material. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and to provide a method for preparing an improved adsorption dehumidification material for a dehumidification wheel. The adsorption dehumidification material for a dehumidification wheel prepared by this method can be used as the core material of the dehumidification wheel, and in particular can have both a higher dehumidification capacity and a lower regeneration temperature, and has properties such as good mechanical strength.

[0006] In order to solve the above technical problems, a technical solution adopted by the present invention is as follows:

[0007] An adsorption dehumidification material for a dehumidification wheel, the adsorption dehumidification material for a dehumidification wheel comprising a substrate and a moisture absorbing layer coated on the substrate, the moisture absorbing layer being formed by coating a composite slurry on the substrate, the composite slurry comprising the following components: sodium polyacrylate, waterborne polyurethane and a solvent; wherein the raw materials of the waterborne polyurethane comprise polyisocyanate, hydrophilic polyol, hydrophilic chain extender, a hydroxyl-containing small molecule chain extender having a molecular weight of less than or equal to 200, and a hydroxyl-containing water-soluble polymer;

[0008] The waterborne polyurethane is prepared by the following method: a polyisocyanate and a hydrophilic polyol are subjected to a first reaction to prepare a polyurethane prepolymer, a hydrophilic chain extender containing a carboxyl group and a hydroxyl-containing small molecule chain extender with a molecular weight of less than or equal to 200 are added, a second reaction is carried out, a hydroxyl-containing water-soluble polymer is added, and a third reaction is carried out to generate the waterborne polyurethane.

[0009] According to some preferred aspects of the present invention, the mass ratio of the polyisocyanate to the hydrophilic polyol is 1:0.2-2.5.

[0010] According to some preferred aspects of the present invention, the polyisocyanate is a combination of one or more selected from toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, modified diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate and hexamethylene diisocyanate.

[0011] According to some preferred aspects of the present invention, the hydrophilic polyol is polyethylene glycol with a molecular weight of 400 to 2000. According to a specific aspect of the present invention, the hydrophilic polyol includes but is not limited to polyethylene glycol 400 (PEG 400), polyethylene glycol 1000 (PEG 1000) or polyethylene glycol 2000 (PEG 2000), which can be commercially obtained.

[0012] According to some preferred aspects of the present invention, the first reaction is carried out in the presence of a catalyst and under the protection of a protective gas at 60-90° C. The catalyst includes dibutyltin dilaurate (DBTDL), and the protective gas may be nitrogen or argon.

[0013] In some embodiments of the present invention, the added amount of the catalyst accounts for 0.2-2% of the added amount of the polyisocyanate.

[0014] In some embodiments of the present invention, the reaction time of the first reaction is 1-4 hours.

[0015] According to some preferred aspects of the present invention, the mass ratio of the polyisocyanate, the hydrophilic chain extender and the hydroxyl-containing small molecule chain extender is 1:0.0.8-0.35:0.1-0.2.

[0016] According to some preferred aspects of the present invention, the hydrophilic chain extender is a combination of one or more selected from 2,2-dimethylolpropionic acid (DMPA), 2,2-dimethylolbutanoic acid (DMBA) and sodium dimethyl 5-sulfoisophthalate (SIPM).

[0017] According to some preferred aspects of the present invention, the hydroxyl-containing small molecule chain extender is a combination of one or more selected from ethylene glycol (EG), 1,4-butanediol (BDO) and diethanolamine (DEA).

[0018] According to some preferred aspects of the present invention, the second reaction is carried out under the protection of a protective gas at 60-90° C., and the protective gas may be nitrogen or argon.

[0019] In some embodiments of the present invention, the reaction time of the second reaction is 1-4 hours.

[0020] According to some preferred aspects of the present invention, the hydroxyl-containing water-soluble polymer is sodium carboxymethyl cellulose (CMC-Na) and / or sodium carboxymethyl starch (CMS-Na).

[0021] In the present invention, the viscosity of the sodium carboxymethyl cellulose at 25°C is 50-200 mpa·s, and the viscosity of the sodium carboxymethyl starch at 25°C is 50-200 mpa·s.

[0022] According to some preferred aspects of the present invention, the third reaction is carried out at 50-80° C. under the protection of a protective gas, and the protective gas may be nitrogen or argon.

[0023] In some embodiments of the present invention, the reaction time of the third reaction is 0.5-1.5h.

[0024] According to some preferred aspects of the present invention, the raw materials of the waterborne polyurethane include, by weight, 100 parts of polyisocyanate, 20-250 parts of hydrophilic polyol, 8-35 parts of hydrophilic chain extender, 10-20 parts of hydroxyl-containing small molecule chain extender with a molecular weight of less than or equal to 200, and 5-50 parts of hydroxyl-containing water-soluble polymer, and optionally 5-15 parts of a neutralizer, wherein the neutralizer includes triethylamine (TEA) and triethanolamine (TEOA).

[0025] According to some specific and preferred aspects of the present invention, when DMPA or DMBA is used as the hydrophilic chain extender containing a carboxyl group, the corresponding neutralizing agent is one of TEA or TEOA, and when SIPM is used as the hydrophilic chain extender containing a carboxyl group, no neutralizing agent is needed.

[0026] According to some preferred aspects of the present invention, the solvent is water.

[0027] According to some preferred aspects of the present invention, the composite slurry is prepared by mixing a sodium polyacrylate solution with a solid content of 5-15wt% and an aqueous polyurethane emulsion with a solid content of 35-45wt%, wherein the sodium polyacrylate solution is prepared by dispersing sodium polyacrylate (PAA-Na) in water, and the aqueous polyurethane emulsion is prepared by emulsifying an aqueous polyurethane dispersed in water, and the feed volume ratio of the sodium polyacrylate solution to the aqueous polyurethane emulsion is 1:1-2.

[0028] In some embodiments of the present invention, the temperature during the neutralization and emulsification is 20-50° C., the neutralization time is 5-20 min, and the emulsification time is 10-60 min.

[0029] Another technical solution provided by the present invention is a method for preparing the above-mentioned adsorption dehumidification material for the dehumidification wheel, the preparation method comprising the following steps:

[0030] The substrate is immersed in the composite slurry and then dried to obtain a product; wherein the immersion time is 0.5-3h and the drying temperature is 50-90°C.

[0031] In some embodiments of the present invention, the substrate includes, but is not limited to, honeycomb glass fibers.

[0032] Another technical solution provided by the present invention is a dehumidification wheel, wherein the dehumidification wheel adopts the above-mentioned adsorption dehumidification material for the dehumidification wheel as the wheel core material.

[0033] Due to the adoption of the above technical solution, the present invention has the following advantages compared with the prior art:

[0034] Based on the problem of high desorption temperature of the wheel core material used in the dehumidification wheel in the prior art, the present invention innovatively selects a waterborne polyurethane (WPU) with excellent adhesion and certain hydrophilicity as a matrix, performs hygroscopic modification on it, so that it obtains excellent hygroscopic performance at the molecular level, specifically by introducing a compounded hydrophilic group to enhance its own hygroscopic performance, and finally introduces PAA-Na with excellent hygroscopic performance through physical blending to further enhance the dehumidification capacity of the material, and the adhesion of WPU enables PAA-Na to better adhere to the carrier, thereby preparing an adsorption dehumidification material for a dehumidification wheel with excellent hygroscopic capacity. At the same time, the adsorption dehumidification material for a dehumidification wheel can also remove surface adsorbed moisture at a lower temperature, thereby obtaining a low-temperature regenerated adsorption dehumidification material whose strength and performance meet the use requirements. DETAILED DESCRIPTION

[0035] The following is a combination of several embodiments of the present invention to better illustrate the technical route and implementation effect of the present invention. The following embodiments are only a few examples of the present invention and are not intended to limit the present invention. Other embodiments obtained by other researchers in the field based on the technical solution of the present invention should fall within the protection scope of the present invention.

[0036] In the following, unless otherwise specified, all raw materials can be purchased from commercial sources or prepared by conventional methods in the art. IPDI is isophorone diisocyanate, purchased from Aladdin Reagent Co., Ltd.;

[0037] PEG 400, PEG 1000, and PEG 2000 were purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0038] CMC-Na was purchased from Aladdin Reagent Co., Ltd. with the brand name C299502; CMS-Na was purchased from Aladdin Reagent Co., Ltd. with the brand name C105666; and sodium polyacrylate was purchased from Aladdin Reagent Co., Ltd. with the brand name S298808.

[0039] Example 1

[0040] 100 parts by mass of IPDI, 90 parts by mass of PEG1000 and 0.5 parts by mass of DBTDL were added to a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and prepolymerized at 90°C under nitrogen protection for 3 hours. Subsequently, 15 parts by mass of DMPA and 15 parts by mass of BDO were added to the four-necked flask, and the chain extension was continued at 90°C under nitrogen protection for 2 hours. After the chain extension was completed, 30 parts by mass of CMC-Na were added, and the modification was carried out at 80°C under nitrogen protection for 1 hour. After the reaction was completed, the system temperature was lowered to 25°C and 11 parts by mass of TEA were added for neutralization for 10 minutes, followed by the addition of 391.5 parts by mass of deionized water and emulsification at 25°C for 30 minutes to obtain an aqueous polyurethane emulsion (WPU emulsion) with a solid content of 40wt%.

[0041] A PAA-Na aqueous solution with a solid content of 10wt% and a WPU emulsion with a solid content of 40wt% were mixed in a volume ratio of 1:1 to obtain a WPU / PAA-Na composite slurry. A honeycomb glass fiber carrier was soaked in the composite slurry for 2h, then purged and dried in flowing hot air at 80°C to constant weight.

[0042] Example 2

[0043] 100 parts by mass of IPDI, 200 parts by mass of PEG2000 and 0.8 parts by mass of DBTDL were added to a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and prepolymerized at 75°C under nitrogen protection for 4 hours. Subsequently, 15 parts by mass of DMBA and 16 parts by mass of DEA were added to the four-necked flask, and the chain was extended at 85°C under nitrogen protection for 2 hours. After the chain extension was completed, 38 parts by mass of CMC-Na were added, and the modification was carried out at 70°C under nitrogen protection for 1.5 hours. After the reaction was completed, the system temperature was lowered to 35°C and 10 parts by mass of TEA were added for neutralization for 15 minutes, followed by the addition of 568.5 parts by mass of deionized water and emulsification at 35°C for 40 minutes to obtain an aqueous polyurethane emulsion (WPU emulsion) with a solid content of 40wt%.

[0044] A PAA-Na aqueous solution with a solid content of 10wt% and a WPU emulsion with a solid content of 40wt% were mixed in a volume ratio of 2:3 to obtain a WPU / PAA-Na composite slurry. A honeycomb glass fiber carrier was soaked in the composite slurry for 3 hours, then purged and dried in flowing hot air at 75°C to constant weight.

[0045] Example 3

[0046] 100 parts by mass of IPDI, 60 parts by mass of PEG400 and 0.5 parts by mass of DBTDL were added to a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and prepolymerized at 70°C under nitrogen protection for 2 hours. Subsequently, 30 parts by mass of SIPM and 10 parts by mass of BDO were added to the four-necked flask, and the chain was extended at 90°C under nitrogen protection for 3 hours. After the chain extension was completed, 35 parts by mass of CMS-Na were added, and the modification was carried out at 75°C under nitrogen protection for 1 hour. After the reaction was completed, the system temperature was reduced to 50°C and 352.5 parts by mass of deionized water were added and emulsified at 50°C for 20 minutes to obtain an aqueous polyurethane emulsion (WPU emulsion) with a solid content of 40wt%.

[0047] A PAA-Na aqueous solution with a solid content of 10wt% and a WPU emulsion with a solid content of 40wt% were mixed in a volume ratio of 1:2 to obtain a WPU / PAA-Na composite slurry. A honeycomb glass fiber carrier was placed in the composite slurry and soaked for 2.5h, then purged and dried in flowing hot air at 70°C to constant weight.

[0048] Comparative Example 1

[0049] 100 parts by mass of IPDI, 100 parts by mass of PEG1000 and 0.5 parts by mass of DBTDL were added to a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and prepolymerized at 90°C under nitrogen protection for 2 hours. Subsequently, 30 parts by mass of SIPM and 12 parts by mass of EG were added to the four-necked flask, and chain extension was performed at 80°C under nitrogen protection for 2 hours. After the reaction was completed, the system temperature was lowered to 25°C and 363 parts by mass of deionized water were added and emulsified at 35°C for 30 minutes to obtain a WPU emulsion with a solid content of 40wt%.

[0050] A PAA-Na aqueous solution with a solid content of 10wt% and a WPU emulsion with a solid content of 40wt% were mixed in a volume ratio of 1:1 to obtain a WPU / PAA-Na composite slurry. A honeycomb glass fiber carrier was soaked in the composite slurry for 2h, then purged and dried in flowing hot air at 80°C to constant weight.

[0051] Comparative Example 2

[0052] The honeycomb glass fiber carrier was immersed in a 10 wt % PAA-Na aqueous solution for 3 h, then purged and dried in flowing hot air at 80° C. to a constant weight.

[0053] Comparative Example 3

[0054] A sample of a commercially available silica gel dehumidification wheel.

[0055] Performance Testing

[0056] The honeycomb dehumidification materials prepared in Examples 1-3 and Comparative Examples 1-3 were cut into the same volume and dried to constant weight, and their moisture absorption rates were measured after adsorption for 15 minutes under the conditions of fixed wind speed (5 m / s) and fixed temperature and humidity (15°C / 95%) (moisture absorption rate = increased mass after adsorption / mass before adsorption). The test results are shown in Table 1, where m0 is the original mass of the dry sample, m1 is the mass of the sample after 15 minutes of adsorption, and △m is the increased mass after adsorption.

[0057] Take some materials prepared by Examples 1-3 and Comparative Examples 1-3, which were adsorbed for 15 min under the above conditions, and measure their desorption rates (desorption rate = mass reduced after desorption / mass increased after adsorption) after desorption for 15 min in desorption winds of fixed wind speed (5 m / s) and different temperatures (60°C / 70°C / 80°C). The test results are shown in Table 2 (desorption temperature is 60°C), Table 3 (desorption temperature is 70°C) and Table 4 (desorption temperature is 80°C), respectively. In the table, m0 is the original mass of the dry sample, m1 is the mass of the sample after adsorption for 15 min, m2 is the mass of the sample after desorption for 15 min, △m1 is the mass increased after adsorption, and △m2 is the mass reduced after desorption.

[0058] Table 1

[0059] Group <![CDATA[m0 / g]]> <![CDATA[m1 / g]]> △m / g Moisture absorption rate / % Example 1 291.5 350.4 58.9 20.2 Example 2 306.9 372.2 65.3 21.3 Example 3 279.7 335.9 56.2 20.1 Comparative Example 1 318.3 351.0 32.7 10.3 Comparative Example 2 179.5 212.0 32.5 18.1 Comparative Example 3 503.2 592.1 88.9 17.7

[0060] Table 2

[0061] Group <![CDATA[m0 / g]]> <![CDATA[m1 / g]]> <![CDATA[m2 / g]]> <![CDATA[△m1 / g]]> <![CDATA[△m2 / g]]> Desorption rate / % Example 1 291.5 350.4 298.8 58.9 51.6 87.6 Example 2 306.9 372.2 319.3 65.3 52.9 81.0 Example 3 279.7 335.9 285.5 56.2 50.4 89.7 Comparative Example 1 318.3 351.0 321.6 32.7 29.4 89.9 Comparative Example 2 179.5 212.0 182.2 32.5 29.8 91.7 Comparative Example 3 503.2 592.1 538.9 88.9 53.2 59.8

[0062] Table 3

[0063]

[0064]

[0065] Table 4

[0066] Group <![CDATA[m0 / g]]> <![CDATA[m1 / g]]> <![CDATA[m2 / g]]> <![CDATA[△m1 / g]]> <![CDATA[△m2 / g]]> Desorption rate / % Example 1 290.7 349.8 293.6 59.1 56.2 95.1 Example 2 306.2 371.7 309.9 65.5 61.8 94.4 Example 3 280.6 337.0 282.9 56.4 54.1 95.9 Comparative Example 1 315.6 347.9 316.8 32.3 31.1 96.3 Comparative Example 2 178.9 211.2 180.0 32.3 31.2 96.6 Comparative Example 3 506.1 595.4 531.8 89.3 63.6 71.2

[0067] By comparing the embodiment with comparative example 1, it can be seen that the dehumidification performance of WPU is significantly improved after hydrophilic modification. The comparison between the embodiment and comparative example 2 shows that when PAA-Na is used alone as the adsorption material, although it has a good adsorption rate, it is affected by the viscosity of the solution and the amount that can be coated on the glass fiber carrier is limited. In addition, the lack of the bonding force of WPU will lead to poor mechanical strength of the material, and the honeycomb carrier is easy to fall apart under stress. Moreover, the comparison between the embodiment and comparative example 3 shows that the desorption rate of the silica gel material at a temperature of 60 to 80°C for 15 minutes is much lower than that of the adsorption dehumidification material prepared by the present invention, and the adsorption dehumidification material prepared by the present invention can reach an adsorption rate of more than 85%. If the adsorption dehumidification material prepared by the present invention is used as the core of the runner, the regeneration energy consumption during the operation of the runner can be significantly reduced.

[0068] The above embodiments are only a part of the embodiments of the present invention. Those skilled in the art can easily implement other embodiments based on the present invention. Therefore, any changes and modifications made without departing from the technical solution of the present invention should fall within the protection scope of the present invention.

Claims

1. A method for preparing an adsorption dehumidification material for a dehumidification wheel, characterized in that: The preparation method comprises: Preparation of waterborne polyurethane emulsion: polyisocyanate and hydrophilic polyol are subjected to a first reaction to prepare polyurethane prepolymer, a hydrophilic chain extender and a hydroxyl-containing small molecule chain extender with a molecular weight of less than or equal to 200 are added, a second reaction is carried out, a hydroxyl-containing water-soluble polymer is added, a third reaction is carried out to generate waterborne polyurethane; and the waterborne polyurethane emulsion is prepared by dispersing the waterborne polyurethane in water and emulsifying the waterborne polyurethane; In the process of preparing waterborne polyurethane, the raw materials of waterborne polyurethane include, by weight: 100 parts of polyisocyanate, 20-250 parts of hydrophilic polyol, 8-35 parts of hydrophilic chain extender, 10-20 parts of hydroxyl-containing small molecule chain extender with a molecular weight of less than or equal to 200, and 5-50 parts of hydroxyl-containing water-soluble polymer, and optionally include 5-15 parts of neutralizer, wherein the neutralizer includes triethylamine and triethanolamine; The hydrophilic polyol is polyethylene glycol with a molecular weight of 400-2000; The hydrophilic chain extender is a combination of one or more selected from 2,2-dimethylol propionic acid, 2,2-dimethylol butyric acid and sodium dimethyl 5-sulfonate isophthalate; The hydroxyl-containing small molecule chain extender is a combination of one or more selected from ethylene glycol, 1,4-butanediol and diethanolamine; The hydroxyl-containing water-soluble polymer is sodium carboxymethyl cellulose and / or sodium carboxymethyl starch; Preparation of sodium polyacrylate solution: dispersing sodium polyacrylate in water to prepare sodium polyacrylate solution; Preparation of composite slurry: mixing sodium polyacrylate solution and aqueous polyurethane emulsion to obtain composite slurry; The substrate is immersed in the composite slurry and then dried to prepare an adsorption dehumidification material for a dehumidification wheel.

2. The method for preparing the adsorption dehumidification material for a dehumidification wheel according to claim 1, characterized in that: The solid content of the aqueous polyurethane emulsion is controlled to be 35-45 wt %, the solid content of the sodium polyacrylate solution is controlled to be 5-15 wt %, and the volume ratio of the sodium polyacrylate solution to the aqueous polyurethane emulsion is 1:1-2.

3. The method for preparing the adsorption dehumidification material for a dehumidification wheel according to claim 1, characterized in that: The first reaction is carried out in the presence of a catalyst, under the protection of a protective gas, at 60-90° C., wherein the catalyst comprises dibutyltin dilaurate; The second reaction is carried out under protective gas protection at 60-90° C.; The third reaction is carried out at 50-80° C. under the protection of protective gas.

4. The method for preparing the adsorption dehumidification material for a dehumidification wheel according to claim 3, characterized in that: In terms of mass percentage, the amount of the catalyst added is 0.2-2% of the amount of the polyisocyanate added; The reaction time of the first reaction is 1-4 hours, the reaction time of the second reaction is 1-4 hours, the reaction time of the third reaction is 0.5-1.5 hours, and the protective gas is nitrogen or argon.

5. The method for preparing the adsorption dehumidification material for a dehumidification wheel according to claim 1, characterized in that: When 2,2-dihydroxymethylpropionic acid or 2,2-dihydroxymethylbutyric acid is used as the hydrophilic chain extender, the corresponding neutralizing agent is one of triethylamine or triethanolamine. When sodium dimethyl isophthalate-5-sulfonate is used as the hydrophilic chain extender, no neutralizing agent is needed.

6. The method for preparing the adsorption dehumidification material for a dehumidification wheel according to claim 1 or 5, characterized in that: The viscosity of the sodium carboxymethyl cellulose at 25°C is 50-200 mPa·s, the viscosity of the sodium carboxymethyl starch at 25°C is 50-200 mPa·s, and the substrate is honeycomb glass fiber.

7. The method for preparing an adsorption dehumidification material for a dehumidification wheel according to claim 1 or 5, characterized in that: The mass ratio of the polyisocyanate to the hydrophilic polyol is 1:0.2-2.5, and the mass ratio of the polyisocyanate, the hydrophilic chain extender and the hydroxyl-containing small molecule chain extender is 1:0.08-0.35:0.1-0.

2.

8. The method for preparing the adsorption dehumidification material for a dehumidification wheel according to claim 1, characterized in that: In the preparation process of the waterborne polyurethane emulsion, the emulsification temperature is 20-50° C. and the emulsification time is 10-60 min.

9. The method for preparing the adsorption dehumidification material for a dehumidification wheel according to claim 1, characterized in that: The soaking time of the soaking is 0.5-3h.

10. The method for preparing an adsorption dehumidification material for a dehumidification wheel according to claim 1, characterized in that: The drying temperature of the drying is 50-90° C., and the drying is carried out in flowing hot air and the drying is carried out to a constant weight.