A bonding powder for diamond matrix and preparation method thereof, and diamond matrix

By using highly reactive bonding powder with core-shell structure during the sintering process of diamond tools, the problems of poor wetting and oxygen influence of bonded metals and diamond and skeleton metals in traditional technology are solved, and efficient bonding of diamond tools is achieved and performance improvements extend service life.

CN115740439BActive Publication Date: 2024-11-19ZHENGZHOU RES INST OF MECHANICAL ENG CO LTD +3
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202211379336.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-11-19
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

During the sintering process, traditional diamond tools have poor wettability of bonded metals, diamond and skeleton metals, resulting in uneven tissue structure, low bond strength, and oxygen in the sintering environment affects performance, resulting in poor tool performance.

Method used

Highly reactive bonding powder with core-shell structure is adopted, the core is Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, and the outer shell is a B-Al composite powder layer. B2O3 is generated by in-situ reaction between B powder and oxygen. , Al powder forms Al2O3 ceramic phase, reduces oxygen content and forms a network-like structure, and improves bonding strength and uniformity.

Benefits of technology

It significantly improves the structural uniformity and bonding strength of diamond tools, extends service life, reduces product defect rate, realizes the metallurgical combination of diamond and skeleton metal, and improves the performance and wear resistance of the tool.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115740439B_ABST
    Figure CN115740439B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of diamond tool matrix, and in particular, relates to a bonding powder for diamond matrix and a preparation method thereof, and a diamond matrix. The bonding powder for diamond matrix of the present invention has a core-shell structure, and the core-shell structure includes a core and an outer shell, the core is Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, and the outer shell is a B-Al composite powder layer formed by B powder coating Al powder; the mass ratio of the core to the outer shell is (5-15):1. The bonding powder of the present invention, through the above-mentioned special core-shell structure design, can reduce inclusions in the matrix, purify the connection area, and improve the bonding strength on the one hand, and can effectively wet the skeleton metal and diamond particles on the other hand, so that the composition and organizational structure of the matrix are more evenly distributed, avoiding component segregation, and improving the bonding strength between the bonding metal and the skeleton metal and diamond. Therefore, the present invention has good application prospects in the field of high-performance diamond matrix preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of diamond tool matrix, and in particular relates to a bonding powder for diamond matrix and a preparation method thereof, and a diamond matrix. Background Art

[0002] Diamond tools are made by sintering a matrix and diamond, where the matrix is ​​divided into a bonding metal and a skeleton metal. When sintering traditional diamond tools, the bonding metal (Cu powder, Zn powder, Sn powder, etc.), the skeleton metal (Ni powder, Fe powder, etc.) and the diamond particles are mixed evenly and then hot-pressed and sintered. During the sintering process, the low-melting-point elements Sn and Zn, which are easily burned, contact and dissolve the Cu in the particle system under the action of the pre-sintering pressure to form a continuous Cu-Sn and Cu-Zn alloy liquid phase. However, due to the poor wettability between the Cu-Sn and Cu-Zn alloy liquid phases and the Fe and C (diamond) particles and the uneven distribution of the two in the system, most of the Cu-Sn and Cu-Zn liquid phases cannot penetrate into the cracks of the Fe and C particles to form an effective bond with them, resulting in an uneven sample structure. Therefore, a large number of Fe and C particles in the system contact each other under the action of the sintering pressure and form an unstable solid phase sintering, which greatly affects the sintering effect and tool performance of the diamond tool. At the same time, during the sintering process, trace amounts of oxygen in the sintering environment and oxygen on the surface of the metal powder cannot be effectively removed, forming inclusions, further affecting the performance of the sintered diamond tools (such as diamond tool bits).

[0003] In order to improve the service life and performance of diamond tools, the diamond tool industry urgently needs to improve the wettability and uniformity of the bonding metal to the diamond and skeleton metal, and reduce the impact of powder and oxygen in the atmosphere on the performance during the sintering process, thereby reducing the product defect rate, achieving effective bonding of diamond and skeleton, and extending their service life.

[0004] For example, a Chinese invention patent with authorization announcement number CN106191625B discloses an iron-based matrix powder for diamond composite blocks, which solves the problem of reduced performance of diamond tools due to the generation of metal oxides during sintering by dispersing nano-aluminum powder in the iron-based matrix powder. However, the aluminum powder added in this method exists as a single particle, and its surface easily reacts with oxygen to generate oxides during the sintering process. The formed aluminum oxide film is relatively dense, and it is difficult for the aluminum in the core to continue to absorb external oxygen to reduce the overall oxygen content. Therefore, its effect on improving the matrix performance is relatively limited.

[0005] Therefore, developing a highly active bonding metal matrix powder that can improve the uniformity, bonding strength and service life of diamond structure has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] In order to solve the above problems, the first purpose of the present invention is to provide a bonding powder for diamond matrix, which is essentially a highly active bonding metal powder, which can solve the technical problems of poor uniformity of the organizational structure formed by the existing matrix bonding materials and the skeleton metal and diamond, high impurity content and low bonding strength.

[0007] The second object of the present invention is to provide a method for preparing bonding powder for diamond matrix, which has simple operation, mild conditions and is suitable for industrial application.

[0008] The third object of the present invention is to provide a diamond matrix, whose matrix components and organizational structure are evenly distributed, which can achieve metallurgical bonding between bonding metal, skeleton metal and diamond, effectively avoid the occurrence of component segregation, and significantly improve the holding force of the matrix on diamond.

[0009] In order to achieve the above object, the bonding powder for diamond matrix of the present invention adopts the technical scheme as follows:

[0010] A bonding powder for a diamond matrix, the bonding powder for a diamond matrix having a core-shell structure, the core-shell structure comprising a core and an outer shell, the core being a Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, the outer shell being a B-Al composite powder layer formed by B powder coating Al powder;

[0011] The Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder is composed of the following raw materials in weight percentage: Sn 10-15%, Zn 20-30%, Ni 1-10%, Ti 0.5-5%, Cr 1-5%, Zr 1-10%, and the balance is Cu; in the B-Al composite powder layer, the mass ratio of B powder to Al powder is 1:(15-20); and the mass ratio of the inner core to the outer shell is (5-15):1.

[0012] The bonding powder for diamond matrix of the present invention has a core-shell structure, wherein the core is Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, the outer shell is a B-Al composite powder layer, and the B-Al in the composite powder layer has a core-shell structure of B powder covering Al powder.

[0013] The present invention adopts the above-mentioned special core-shell structure bonding powder. When it is used for sintering preparation of the matrix, the B powder in the outer shell will preferentially react with the oxygen in the sintering atmosphere and the surface of the skeleton metal powder in situ to generate B2O3. The generated B2O3 will further react with various oxides on the surface of the alloy (the oxygen adsorbed on the surface of the Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder will cause powder oxidation during heating to form copper oxide, zinc oxide, tin oxide, chromium oxide and other oxides), thereby achieving the purpose of reducing inclusions in the matrix, purifying the connection area and improving the bonding strength.

[0014] As the sintering process proceeds, the Al powder in the shell will generate Al2O3 ceramic phase after in-situ oxidation. The Al2O3 and B2O3 generated on the surface further react to form a composite salt, which promotes the new Al to leak out and further react with oxygen, further reducing the oxygen content in the entire atmosphere. At the same time, the Al2O3 ceramic phase generated can further enhance the wear resistance and bonding strength of the matrix.

[0015] As the sintering progresses, when the sintering temperature reaches the liquidus temperature of the Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, the alloy powder will instantly transform into a liquid phase, wetting the Fe, Ni and other skeleton powders and diamond particles. Ultimately, the Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy can form a continuous network structure, fully wrapping and bonding the Fe, Ni and other skeleton particles and diamond particles. The formation of this network structure makes the composition and organizational structure of the matrix more evenly distributed, avoiding the occurrence of component segregation.

[0016] Furthermore, the matrix composition designed in the present invention contains the same elements as those in the skeleton metal, and has better affinity with the skeleton metal and is easy to combine with each other, thereby effectively improving the bonding strength between the bonding metal and the skeleton metal and diamond, and improving the holding force of the matrix on the diamond, which is more conducive to improving the service life of the diamond tool.

[0017] The preferred solution of the present invention is introduced below. Based on the consideration of improving the bonding strength of the bonding powder to the skeleton metal and diamond, the uniformity of the tissue distribution and the stability, preferably, the particle size of the bonding powder for the diamond matrix is ​​150-300 μm.

[0018] Further preferably, the mass ratio of the core to the shell is (8-10):1; more preferably, the mass ratio of the core to the shell is 9:1.

[0019] The present invention provides a method for preparing bonding powder for diamond matrix, and the specific scheme is as follows:

[0020] The method for preparing bonding powder for diamond matrix comprises the following steps:

[0021] (1) ball milling Al powder, B powder and a dispersant, and then drying to obtain a B-Al composite powder;

[0022] (2) The B-Al composite powder, the pre-alloyed powder of Cu-Zn-Sn-Ni-Ti-Cr-Zr and the dispersant are ball-milled, and then dried and screened to obtain the bonding powder for the diamond matrix.

[0023] The method for preparing bonding powder for diamond matrix provided by the present invention is a purely physical preparation method, which can avoid the risk of environmental pollution caused by chemical processes, and has mild reaction conditions and simple operation, and is suitable for large-scale production of bonding powder for matrix.

[0024] Preferably, in step (1), the purity of the Al powder and the B powder is ≥ 99.9%. The use of high-purity Al and B powder raw materials can avoid the influence of further introduction of inclusions on the sintering process.

[0025] By controlling the particle size of the raw material powder, the B powder can effectively cover the Al powder by relying on the size effect, thereby ensuring the preparation quality of the bonding powder, thereby improving the bonding powder's effect on removing inclusions during the matrix sintering process and improving the bonding strength. Preferably, in step (1), the average particle size of the B powder is less than 10 μm; the average particle size of the Al powder is 20 to 30 μm.

[0026] Further preferably, in step (2), the average particle size of the pre-alloyed powder is 100 to 250 μm. The preparation of the pre-alloyed powder can be carried out by conventional techniques in the art. For example, Cu, Zn, Sn, Ni, Ti, Cr, and Zr powders can be taken in mass proportions and prepared by an atomization method to obtain the pre-alloyed powder.

[0027] The Al powder and the B powder are mixed and ball-milled to form a B-Al composite powder having a core-shell structure of Al powder coated with B powder. In order to ensure the subsequent sintering effect of the composite powder, preferably, the average particle size of the B-Al composite powder is ≤50 μm.

[0028] As a further preferred embodiment of the present invention, in steps (1) and (2), the dispersant is one or both of ethanol and acetone. By adding the dispersant, the sphericity of the prepared B-Al composite powder with a core-shell structure and the bonding powder for the diamond matrix can be improved, and the powder adhesion can be avoided.

[0029] More preferably, the amount of dispersant added is 2-5% of the total mass of the raw materials in the system. The amount of dispersant added within the above range can avoid powder adhesion and ensure the uniformity of powder dispersion, thereby further improving the sphericity of the prepared bonded powder.

[0030] Furthermore, in steps (1) and (2), the rotation speed of the ball mill is 300-500 r / min, the ball milling time is 20-40 h, and the ball-to-material ratio of the ball mill is (18-22):1. More preferably, the rotation speed of the ball mill is 400 r / min, the ball milling time is 20 h, and the ball-to-material ratio of the ball mill is 20:1. The ball milling process can use a medium suitable for the ball milling process of metal powders, such as agate balls as ball milling media. In actual operation, the ball milling process can be carried out in an agate jar, such as an agate ball milling jar.

[0031] In a preferred embodiment of the present invention, in steps (1) and (2), the drying is performed under vacuum conditions. Preferably, the vacuum degree of the vacuum conditions is greater than or equal to -0.1 MPa. By adopting vacuum conditions, oxidation of the powder can be prevented. Further preferably, the drying temperature is 100 to 120° C., and the drying time is 2 to 10 hours.

[0032] In step (2), the screening is performed according to the particle size actually required to obtain a bonding powder of a core-shell structure with a required particle size.

[0033] The technical scheme adopted by the diamond matrix of the present invention is as follows:

[0034] A diamond matrix is ​​prepared by uniformly mixing a skeleton metal and a bonding metal and then hot pressing and sintering them; the skeleton metal is composed of Fe, Cu and Ni, and the mass percentage of each raw material in the skeleton metal to the diamond matrix is: Fe 40%-45%, Cu 15%-20%, Ni 3%-10%; the bonding metal is the bonding powder for the diamond matrix as described above, and the mass percentage of the bonding powder for the diamond matrix to the diamond matrix is ​​25%-35%.

[0035] The diamond matrix of the present invention belongs to an iron-based matrix material and adopts a bonding powder for the diamond matrix with a special structure, which overcomes the problems of easy burning, easy inclusion, and inability to penetrate into the cracks between Fe, Cu and Ni particles to form effective bonding with them, thereby causing uneven sample structure, poor bonding strength and poor performance of diamond tools.

[0036] Further preferably, the raw material composition of the diamond matrix is, by mass percentage, 45% Fe, 18% Cu, 5% Ni and 32% of the bonding powder for the diamond matrix as described above.

[0037] As a preferred solution of the present invention, a material in which the skeleton metal and the bonding metal are evenly mixed is placed in a mold and then hot-pressed and sintered. The mold can be selected appropriately according to the shape requirements of the actual matrix.

[0038] Further preferably, the mixing is performed by a vacuum mixer, and the mixing time is ≥ 2 hours. Further, the vacuum mixer can be a V-shaped vacuum mixer, or other types of mixers.

[0039] Preferably, the hot pressing sintering temperature is 700-750°C, the pressure is 18-22 MPa, and the heat preservation and pressure holding time is 5-10 minutes. More preferably, the hot pressing sintering temperature is 750°C, the pressure is 20 MPa, and the heat preservation and pressure holding time is 5 minutes.

[0040] More preferably, the hot pressing sintering is performed under vacuum conditions, and the vacuum degree of the vacuum conditions is equal to or higher than -0.1 MPa. By adopting the vacuum conditions, oxidation of the matrix material can be reduced.

[0041] Compared with the prior art, the beneficial effects of the present invention are:

[0042] (1) The bonding powder for diamond matrix provided by the present invention has a special core-shell structure with a composite layer. During the sintering process of the matrix, the outer layer of the core-shell structure will react with oxygen in the matrix and the atmosphere in situ deoxidation. B in the shell layer will be pre-combined with oxygen to form B2O3, and B2O3 will continue to react with the oxide in the powder to purify the connection area and improve the bonding strength; Al in the shell layer will react with oxygen to form Al2O3, and the Al2O3 generated on the surface will further react with B2O3 to form a composite salt, which will cause new Al to leak out and further react with oxygen, further reducing the oxygen content in the entire atmosphere. At the same time, the Al2O3 ceramic phase generated will further enhance the wear resistance and strength of the matrix.

[0043] (2) The diamond matrix bonding powder of the present invention uses a Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder of a specific composition as the core. When the sintering temperature reaches the liquidus temperature of the alloy powder, the Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy can form a continuous network structure, effectively wetting the skeleton powders such as Fe and Ni and the diamond particles. In addition, the alloy powder and the skeleton metal have the same elements, and have a better affinity with the skeleton metal and are easy to combine with each other. Therefore, the skeleton particles such as Fe and Ni and the diamond particles can be effectively wrapped and bonded to avoid component segregation, so that the composition and organizational structure of the matrix are more evenly distributed, and the metallurgical bonding of the bonding metal with the skeleton metal and the diamond is achieved, thereby improving the bonding strength between the matrix material and the diamond and improving the holding force of the matrix on the diamond.

[0044] (3) The bonding powder for the diamond matrix of the present invention is prepared by a physical method, which is green and safe, and is convenient for the industrial production and application of diamond matrix. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a schematic structural diagram of the bonding powder for diamond matrix of the present invention;

[0046] Figure 2 This is a microscopic morphology of a diamond matrix obtained by sintering the diamond matrix of Example 1 of the present invention with bonding powder;

[0047] Figure 3 This is a fracture morphology diagram of a diamond tool obtained by sintering the diamond matrix of Example 1 of the present invention using bonding powder. DETAILED DESCRIPTION

[0048] The technical solution of the present invention is further described below in conjunction with specific implementation modes, but does not constitute a limitation to the present invention.

[0049] The bonding powder for diamond matrix of the present invention has a structural schematic diagram as shown in Figure 1 As shown, it has a core-shell structure, the core is Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, and the shell is a B-Al composite powder layer formed by B powder coating Al powder.

[0050] In the following examples, the specific conditions not specified are all carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or raw materials used in the following examples, unless otherwise specified, are conventional products obtained from commercial channels.

[0051] 1. Embodiment of bonding powder for diamond matrix

[0052] Example 1

[0053] The bonding powder for diamond matrix of this embodiment has a core-shell structure, wherein the core of the core-shell structure is Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, and the outer shell is a B-Al composite powder layer formed by B powder coating Al powder;

[0054] The Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder is composed of the following raw materials in weight percentage: Sn 15%, Zn 25%, Ni 5%, Ti 2%, Cr 3%, Zr 5%, and the balance is Cu; in the B-Al composite powder layer, the mass ratio of B powder to Al powder is 1:15; the mass ratio of the inner core to the outer shell is 9:1; and the particle size of the bonding powder for the diamond matrix is ​​150-200 μm.

[0055] Example 2

[0056] The bonding powder for diamond matrix of this embodiment has a core-shell structure, wherein the core of the core-shell structure is Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, and the outer shell is a B-Al composite powder layer formed by B powder coating Al powder;

[0057] The Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder is composed of the following raw materials in weight percentage: Sn 10%, Zn 30%, Ni 10%, Ti 5%, Cr 1%, Zr 10%, and the balance is Cu; in the B-Al composite powder layer, the mass ratio of B powder to Al powder is 1:18; the mass ratio of the inner core to the outer shell is 5:1; and the particle size of the bonding powder for the diamond matrix is ​​150-200 μm.

[0058] Example 3

[0059] The bonding powder for diamond matrix of this embodiment has a core-shell structure, wherein the core of the core-shell structure is Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, and the outer shell is a B-Al composite powder layer formed by B powder coating Al powder;

[0060] The Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder is composed of the following raw materials in weight percentage: Sn 12%, Zn 20%, Ni 1%, Ti 0.5%, Cr 5%, Zr 1%, and the balance is Cu; in the B-Al composite powder layer, the mass ratio of B powder to Al powder is 1:20; the mass ratio of the inner core to the outer shell is 15:1; and the particle size of the bonding powder for the diamond matrix is ​​200-250 μm.

[0061] 2. Example of a method for preparing bonding powder for diamond matrix

[0062] Example 4

[0063] The method for preparing the bonding powder for diamond matrix of the present embodiment is to prepare the bonding powder for diamond matrix of embodiment 1, and the specific process comprises the following steps:

[0064] (1) Ball milling Al powder, B powder and dispersant, and then drying to obtain B-Al composite powder; wherein the purity of Al powder and B powder is ≥99.9%; the average particle size of B powder is <10μm; the average particle size of Al powder is 20-30μm; the average particle size of B-Al composite powder after ball milling is ≤50μm. In this step, the dispersant is anhydrous ethanol, the amount added is 3% of the total mass of the mixed powder, the ball milling speed is 400r / min, the time is 20h, the ball-to-material ratio is 20:1; the drying vacuum degree is -0.1MPa, the drying temperature is 120℃, and the drying time is 2h;

[0065] (2) The B-Al composite powder and the pre-alloyed powder of Cu-Zn-Sn-Ni-Ti-Cr-Zr (average particle size of 100-250 μm) were mixed in a ratio of 1:9 by mass and loaded into an agate pot containing agate balls, and then anhydrous ethanol as a dispersant was added for ball milling (the amount of anhydrous ethanol added was 3% of the total mass of the mixed powder), the speed of the ball milling was 400 r / min, the time was 20 h, and the ball-to-material ratio was 20:1; after ball milling, the material was placed in a vacuum drying oven for drying, the vacuum degree was -0.1 MPa, the drying temperature was 120°C, and the drying and heat preservation time was 2 h. After drying, the obtained powder was placed in a standard rotary vibrating screen for particle size screening to obtain a bonding powder for a core-shell structure diamond matrix with a particle size of 150-200 μm.

[0066] Example 5

[0067] The method for preparing the bonding powder for diamond matrix of this embodiment is to prepare the bonding powder for diamond matrix of embodiment 2. The specific process is the same as that of embodiment 1 except that the raw material ratio is different.

[0068] Example 6

[0069] The method for preparing the bonding powder for diamond matrix of this embodiment is to prepare the bonding powder for diamond matrix of embodiment 3. The specific process is the same as that of embodiment 1 except that the raw material ratio is different.

[0070] 3. Embodiment of diamond matrix

[0071] Example 7

[0072] The diamond matrix of this embodiment is prepared by hot pressing and sintering after the skeleton metal and the bonding metal are evenly mixed; the skeleton metal is composed of Fe, Cu, and Ni, and the mass percentage of each raw material in the diamond matrix is: Fe 45%, Cu 18%, and Ni 5%; the bonding metal is the bonding powder for the diamond matrix of Example 1, and the mass percentage of the bonding powder for the diamond matrix in the diamond matrix is ​​32%. Among them, the mixing of the raw materials is to mix the materials in a vacuum mixer for 2 hours; the hot pressing and sintering is to load the mixed materials into a preset mold and process them by vacuum hot pressing and sintering, the vacuum degree of vacuum hot pressing and sintering is -0.1MPa, the temperature of hot pressing and sintering is 750℃, the pressure of hot pressing and sintering is 20MPa, and the heat preservation and pressure holding time of hot pressing and sintering is 5min.

[0073] Example 8

[0074] The diamond matrix of this embodiment is prepared by hot pressing and sintering after the skeleton metal and the bonding metal are evenly mixed; the skeleton metal is composed of Fe, Cu, and Ni, and the mass percentage of each raw material in the diamond matrix is: Fe 43%, Cu 20%, and Ni 3%; the bonding metal is the bonding powder for the diamond matrix of Example 2, and the mass percentage of the bonding powder for the diamond matrix in the diamond matrix is ​​34%. Among them, the mixing of the raw materials is to mix the materials in a vacuum mixer for 2 hours; the hot pressing and sintering is to load the mixed materials into a preset mold and process them by vacuum hot pressing and sintering, the vacuum degree of vacuum hot pressing and sintering is -0.1MPa, the temperature of hot pressing and sintering is 750℃, the pressure of hot pressing and sintering is 20MPa, and the heat preservation and pressure holding time of hot pressing and sintering is 5min.

[0075] Example 9

[0076] The diamond matrix of this embodiment is prepared by hot pressing and sintering after the skeleton metal and the bonding metal are evenly mixed; the skeleton metal is composed of Fe, Cu, and Ni, and the mass percentage of each raw material in the diamond matrix is: Fe 40%, Cu 15%, and Ni 10%; the bonding metal is the bonding powder for the diamond matrix of Example 3, and the mass percentage of the bonding powder for the diamond matrix in the diamond matrix is ​​35%. Among them, the mixing of the raw materials is to mix the materials in a vacuum mixer for 2 hours; the hot pressing and sintering is to load the mixed materials into a preset mold and process them by vacuum hot pressing and sintering, the vacuum degree of vacuum hot pressing and sintering is -0.1MPa, the temperature of hot pressing and sintering is 750℃, the pressure of hot pressing and sintering is 20MPa, and the heat preservation and pressure holding time of hot pressing and sintering is 5min.

[0077] 4. Comparative Proportion

[0078] Comparative Example 1

[0079] The bonding metal of this comparative example is a Cu-Zn-Sn-Ni-Ti-Cr-Zr mixed elemental powder, with the composition of Sn 15%, Zn 25%, Ni 5%, Ti 2%, Cr 3%, Zr 5%, and the balance is Cu.

[0080] The diamond matrix of this comparative example is prepared by hot pressing and sintering after the skeleton metal and the binding metal of comparative example 1 are evenly mixed; the skeleton metal is composed of Fe, Cu, and Ni, and the mass percentage of each raw material in the diamond matrix is: Fe 45%, Cu 18%, Ni 5%; the mass percentage of the binding metal in the diamond matrix is ​​32%. Among them, the mixing of the raw materials is to mix the materials in a vacuum mixer for 2 hours; the hot pressing and sintering is to put the mixed materials into a preset mold and process them by vacuum hot pressing and sintering, the vacuum degree of vacuum hot pressing and sintering is -0.1MPa, the temperature of hot pressing and sintering is 750℃, the pressure of hot pressing and sintering is 20MPa, and the heat preservation and pressure holding time of hot pressing and sintering is 5min.

[0081] Comparative Example 2

[0082] The bonding metal of this comparative example is substantially the same in composition and preparation process as the bonding powder for diamond matrix of Example 1, with the only difference being that the raw material B powder is omitted in the corresponding bonding powder structure and preparation process.

[0083] The diamond matrix of this comparative example is substantially the same in composition and preparation process as that of Example 7, with the only difference being that the bonding metal of Comparative Example 2 is used instead of the bonding metal of Example 1.

[0084] Comparative Example 3

[0085] The bonding metal of this comparative example is substantially the same in composition and preparation process as the bonding powder for diamond matrix of Example 1, with the only difference being that the raw material Al powder is omitted in the corresponding bonding powder structure and preparation process.

[0086] The diamond matrix of this comparative example is substantially the same in composition and preparation process as that of Example 7, with the only difference being that the bonding metal of Comparative Example 3 is used instead of the bonding metal of Example 1.

[0087] 5. Test Examples

[0088] Test Example 1 Material Structure Characterization

[0089] The cross-sectional morphology of the diamond matrix obtained from the bonding powder of Example 1 and Comparative Example 1 was analyzed using a Phenom XL scanning electron microscope. The results are as follows: Figure 2 The appearance of the diamond matrix obtained by sintering the diamond matrix obtained by bonding the powders of Example 1 and Comparative Example 1 (i.e., the diamond matrix of Example 7 and Comparative Example 1) was further analyzed by scanning electron microscopy. The results are as follows: Figure 3 As shown. The volume ratio of diamond matrix to diamond sintering raw materials is 7:3, and the parameters of the sintering process are: it takes 5 minutes to heat the sintering material from room temperature to 400°C, 2 minutes to heat from 400°C to 500°C, then keep it at 500°C for 2 minutes, and then it takes 3 minutes to heat from 500°C to 750°C, and then keep it at 750°C for 5 minutes, and then cool it down for morphological characterization.

[0090] Figure 2 middle, Figure 2 a is the cross-sectional morphology of the matrix obtained by sintering the bonding metal obtained from the conventional single substance powder in Comparative Example 1, Figure 2 b is the cross-sectional morphology of the diamond matrix obtained by sintering the bonding powder of Example 1.

[0091] Depend on Figure 2 It can be seen that the matrix prepared by the bonding powder provided by the present invention has small dimples and no obvious broken hard phase particles, while the traditional matrix of comparative example 1 has more hard phase particles and the material tissue distribution shows obvious unevenness, resulting in a decrease in its flexural strength.

[0092] Figure 3 middle, Figure 3 The left picture shows the appearance of the diamond material obtained after sintering the conventional single powder mixed with bonding metal and diamond in Comparative Example 1. Figure 3 The right picture shows the appearance of the diamond material obtained after sintering the bonding powder for the diamond matrix of Example 1 with diamond.

[0093] Depend on Figure 3It can be seen that the matrix material obtained by sintering the material of the present invention has better bonding performance with diamond. Figure 3 The diamond surface in the right picture is rough, with block peeling involved in the reaction. The diamond surface is attached with flaky and granular matrix alloy, and the diamond leakage height reaches about half. It can be seen that the bonding of the matrix to the diamond of the present invention is no longer a simple mechanical inlay, but forms a tight metallurgical bond.

[0094] Test Example 2 Material Performance Test

[0095] Adding diamond particles to the matrix will lead to a decrease in the flexural strength of the sample. The holding force of the matrix on diamond is generally expressed by the flexural strength loss rate η of the powder sintered matrix on diamond particles. The lower the flexural strength loss rate, the higher the holding force of the matrix on diamond and the better the material bonding performance. The calculation formula of the flexural strength loss rate η is as follows:

[0096] η=[(σ1-σ2) / σ1]×100%

[0097] In the formula, σ1 is the flexural strength of the sintered matrix without diamond; σ2 is the flexural strength of the sintered matrix containing diamond particles.

[0098] The bending strength test was carried out in accordance with GB / T 232-2010. The specific test results of the bending strength of the diamond matrix obtained by sintering Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Table 1.

[0099] Table 1 Bending strength of sintered diamond matrix

[0100]

[0101] As shown in Table 1, compared with the matrix formed by using simple powder as bonding metal in the prior art (Comparative Example 1) and the matrix formed by using a single B or Al coating layer bonding metal (Comparative Examples 2-3), the present invention can effectively improve the wettability and uniform dispersion of diamond and skeleton metal through a specific core-shell structure design, thereby significantly improving the bending strength before and after the matrix and diamond are combined, achieving effective metallurgical bonding of diamond and skeleton, effectively improving the holding force of the matrix on diamond, and improving the material bonding performance. The improvement of diamond holding force and bonding performance is of great significance to the reduction of diamond product defect rate and the improvement of diamond tool service life.

[0102] In summary, the bonding powder for diamond matrix provided by the present invention, through a special core-shell structure design, can effectively solve the technical problems of poor uniformity of the organizational structure formed between the existing matrix bonding materials and the skeleton metal and diamond, high impurity content, and low bonding strength, and has good application prospects in the field of preparation of high-performance diamond matrix.

Claims

1. A bonding powder for diamond matrix, characterized in that: The bonding powder for diamond matrix has a core-shell structure, the core-shell structure comprises a core and an outer shell, the core is Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder, and the outer shell is a B-Al composite powder layer formed by B powder coating Al powder; The Cu-Zn-Sn-Ni-Ti-Cr-Zr alloy powder is composed of the following raw materials in weight percentage: Sn 10-15%, Zn 20-30%, Ni 1-10%, Ti 0.5-5%, Cr 1-5%, Zr 1-10%, and the balance is Cu; In the B-Al composite powder layer, the mass ratio of B powder to Al powder is 1:(15-20); The mass ratio of the inner core to the outer shell is (5-15):

1.

2. The bonding powder for diamond matrix according to claim 1, characterized in that: The particle size of the bonding powder for the diamond matrix is ​​150-300 μm.

3. A method for preparing a bonding powder for a diamond matrix as claimed in claim 1, characterized in that: The following steps are involved: (1) ball milling Al powder, B powder and a dispersant, and then drying to obtain a B-Al composite powder; (2) The B-Al composite powder, the pre-alloyed powder of Cu-Zn-Sn-Ni-Ti-Cr-Zr and the dispersant are ball-milled, and then dried and screened to obtain the bonding powder for the diamond matrix.

4. The method for preparing bonding powder for diamond matrix according to claim 3, characterized in that: In step (1), the purity of the Al powder and the B powder is ≥99.9%; the average particle size of the B powder is <10 μm; the average particle size of the Al powder is 20-30 μm; and the average particle size of the B-Al composite powder is ≤50 μm.

5. The method for preparing bonding powder for diamond matrix according to claim 3, characterized in that: In steps (1) and (2), the dispersant is one or both of ethanol and acetone.

6. The method for preparing bonding powder for diamond matrix according to claim 3, characterized in that: In step (2), the average particle size of the pre-alloyed powder is 100 to 250 μm.

7. The method for preparing a bonding powder for a diamond matrix according to any one of claims 3 to 6, characterized in that: In steps (1) and (2), the rotation speed of the ball mill is 300-500 r / min, the ball milling time is 20-40 h, and the ball-to-material ratio of the ball mill is (18-22):

1.

8. The method for preparing a bonding powder for a diamond matrix according to any one of claims 3 to 6, characterized in that: In steps (1) and (2), the drying is carried out under vacuum conditions.

9. A diamond matrix, characterized in that: The diamond matrix is ​​prepared by uniformly mixing a skeleton metal and a bonding metal and then hot pressing and sintering; the skeleton metal is composed of Fe, Cu and Ni, and the mass percentage of each raw material in the skeleton metal to the diamond matrix is: Fe 40% to 45%, Cu 15% to 20%, Ni 3% to 10%; the bonding metal is the bonding powder for the diamond matrix according to claim 1 or 2, and the mass percentage of the bonding powder for the diamond matrix to the diamond matrix is ​​25% to 35%.

10. The diamond matrix according to claim 9, characterized in that: The temperature of the hot pressing sintering is 700-750° C., the pressure is 18-22 MPa, and the heat preservation and pressure holding time is 5-10 minutes.

Citation Information

Patent Citations

  • Iron-based matrix powder for diamond composite blocks and its application

    CN106191625B

  • Copper powder for electrically conductive paste, and electrically conductive paste

    CN101896629A

  • Filling-type sintered diamond drill bit and manufacturing method thereof

    CN103821456A

  • Carcass composition, diamond segment adopting same and preparation method thereof

    CN108342633A

  • Low-fusion cladding alloy powder and preparation method thereof and iron-based diamond matrix