Poly(lactic acid-b-3-hydroxypropionic acid) block copolymer having excellent tensile strength and articles containing the same

By introducing an appropriate amount of 3-hydroxypropionic acid monomer into polylactic acid, poly(lactic acid-b-3-hydroxypropionic acid) block copolymer is prepared, and the problems of insufficient impact resistance and tensile strength of polylactic acid are solved, and the problem of insufficient impact resistance and tensile strength of polylactic acid is achieved. Performance improvements and expanded scope of application.

CN115803359BActive Publication Date: 2024-11-22LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280005484.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-02-24
Filing Date
2022-02-24
Publication Date
2024-11-22
Estimated Expiration
2042-02-24

AI Technical Summary

Technical Problem

Polylactic acid has insufficient impact resistance, heat resistance and tensile strength, which limits its application range, and the introduction of 3-hydroxypropionic acid will lead to deterioration of inherent physical properties when it is uncontrolled.

Method used

Poly(lactic acid-b-3-hydroxypropionic acid) block copolymer is prepared by introducing an appropriate amount of 3-hydroxypropionic acid monomer into polylactic acid, controlling its introduction degree to improve tensile strength and elongation while maintaining poly The inherent physical properties of lactic acid are prepared using lactide ring-opening polymerization reaction and specific catalysts.

Benefits of technology

The tensile strength of polylactic acid has been improved to above 30MPa, expanding its application field, while maintaining the inherent physical properties of polylactic acid, and providing products with excellent tensile strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004040899950000021
    Figure BDA0004040899950000021
  • Figure BDA0004040899950000061
    Figure BDA0004040899950000061
  • Figure BDA0004040899950000071
    Figure BDA0004040899950000071
Patent Text Reader

Abstract

Provided is a poly(lactic acid-b-3-hydroxypropionic acid) block copolymer, wherein various physical properties of polylactic acid such as tensile strength are improved by introducing monomers from 3-hydroxypropionic acid into polylactic acid, thereby expanding its application field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application is based on and claims the priority of Korean Patent Application No. 10-2021-0024928 filed on February 24, 2021 and Korean Patent Application No. 10-2022-0024171 filed on February 24, 2022, respectively, and the disclosures of these two patent applications are incorporated herein by reference in their entirety.

[0003] The present invention relates to a poly (lactic acid-b-3-hydroxypropionic acid) block copolymer having excellent tensile strength and a product containing the same. Background Art

[0004] Polylactic acid (PLA) is a plant-derived resin obtained from plants such as corn, etc., and has attracted widespread attention as an excellent environmentally friendly material due to its biodegradable properties. Unlike existing commonly used petroleum-based resins such as polystyrene resins, polyvinyl chloride resins, polyethylene, etc., polylactic acid has the effects of preventing the depletion of petroleum resources and inhibiting carbon dioxide emissions, so it can reduce environmental pollution, which is a disadvantage of petroleum-based plastic products. Since environmental pollution problems caused by waste plastics, etc. have become social problems, efforts are being made to expand the application range of polylactic acid to products using conventional plastics (petroleum-based resins), such as food packaging materials and containers, electronic product housings, etc.

[0005] However, compared with existing petroleum-based resins, polylactic acid has poor impact resistance and heat resistance, so it has a limited application range. In addition, polylactic acid has weak tensile strength and poor elongation performance and exhibits brittleness, so polylactic acid has limitations as a general-purpose resin.

[0006] In order to improve the above-mentioned shortcomings, copolymers containing other repeating units in polylactic acid have been studied. In particular, 3-hydroxypropionic acid as a comonomer has received attention in order to improve elongation. However, polylactic acid exhibits different physical properties depending on the degree of introduction of 3-hydroxypropionic acid. When the degree of introduction of 3-hydroxypropionic acid is not controlled, it is understood that the inherent physical properties of polylactic acid deteriorate.

[0007] Therefore, the present invention aims to provide a block copolymer having improved physical properties such as tensile strength, etc., while maintaining the inherent physical properties of polylactic acid by controlling the degree of introduction of a monomer derived from 3-hydroxypropionic acid. Summary of the invention

[0008] Technical issues

[0009] Provided are a copolymer having improved physical properties such as tensile strength, etc. while maintaining the inherent properties of polylactic acid; and an article comprising the copolymer.

[0010] Technical Solution

[0011] To achieve the above object, a poly (lactic acid-b-3-hydroxypropionic acid) block copolymer represented by the following formula 1 is provided, wherein the tensile strength of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer is 30 MPa or more:

[0012] [Formula 1]

[0013]

[0014] In formula 1,

[0015] m is an integer from 100 to 1000, and

[0016] n is an integer from 500 to 4000.

[0017] As used herein, the term "poly(lactic acid-b-3-hydroxypropionic acid) block copolymer" is a block copolymer obtained by polymerizing monomers derived from lactic acid and monomers derived from 3-hydroxypropionic acid, as represented by Formula 1, which refers to a block copolymer in which various physical properties of polylactic acid such as tensile strength, etc. are improved by introducing monomers derived from 3-hydroxypropionic acid.

[0018] When the monomer from 3-hydroxypropionic acid is introduced as a comonomer of polylactic acid, various physical properties of polylactic acid can be improved, but the physical properties exhibited will be different depending on the degree of introduction. Therefore, in the present invention, the degree of introduction of the monomer from 3-hydroxypropionic acid can be controlled to improve physical properties such as tensile strength, etc., while maintaining the inherent physical properties of polylactic acid.

[0019] Preferably, m is 250 to 650. m represents the number of repetitions of the monomer derived from 3-hydroxypropionic acid. When the monomer derived from 3-hydroxypropionic acid is introduced within the above range, physical properties such as tensile strength can be improved while maintaining the inherent physical properties of polylactic acid. More preferably, m is 260 or more, 270 or more, or 280 or more; and 640 or less, 600 or less, 500 or less, or 400 or less.

[0020] Preferably, n is 600 to 1400. n represents the number of repetitions of the monomer derived from lactic acid. More preferably, n is 700 or more, 800 or more, 900 or more, or 1000 or more; and 1300 or less or 1200 or less.

[0021] In addition, in the present invention, the relative ratio of the monomers is very important, and preferably, m / n is 0.20 to 0.60. Within the above m / n range, physical properties such as tensile strength can be improved while maintaining the inherent physical properties of polylactic acid. More preferably, m / n is 0.21 or more, 0.22 or more, 0.23 or more, 0.24 or more, or 0.25 or more; and 0.55 or less, 0.50 or less, 0.45 or less, 0.40 or less, 0.35 or less, or 0.30 or less.

[0022] The tensile strength of poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is more than 30MPa. The method for measuring tensile strength will be described in detail in the embodiment described later. Preferably, the tensile strength of poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is more than 31MPa, more than 32MPa, more than 33MPa, more than 34MPa, more than 35MPa, more than 36MPa, more than 37MPa, more than 38MPa, more than 39MPa or more than 40MPa. Meanwhile, when numerical value is higher, tensile strength is more excellent. However, when numerical value is too high, the application field of copolymer can be restricted. From this point of view, the tensile strength of poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is preferably less than 60MPa. More preferably, the tensile strength of the poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is 59 MPa or less, 58 MPa or less, 57 MPa or less, 56 MPa or less, 55 MPa or less, 54 MPa or less, 53 MPa or less, 52 MPa or less, 51 MPa or less or 50 MPa or less.

[0023] Preferably, the elongation of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is 30% to 250%. The method for measuring elongation will be described in detail in the embodiment described later. Preferably, the elongation of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is more than 40%, more than 50%, more than 60%, more than 70%, more than 80%, more than 90%, more than 100%, more than 110%, more than 120%, more than 130%, more than 140%, more than 150%, more than 160%, more than 170%, more than 180%, more than 190% or more than 200%. In addition, preferably, the elongation of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is less than 240%, less than 230%, less than 220% or less than 210%.

[0024] Furthermore, the tensile modulus of the poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is preferably 1.0 GPa to 2.0 GPa. The method of measuring the tensile modulus will be described in detail in the examples described later.

[0025] In addition, the weight average molecular weight of the poly (lactic acid -b-3-hydroxypropionic acid) block copolymer according to the present invention is preferably 50,000 to 350,000. More preferably, the weight average molecular weight of the poly (lactic acid -b-3-hydroxypropionic acid) block copolymer is 60,000 or more, 70,000 or more, 80,000 or more, 90,000 or more, 100,000 or more, 110,000 or more, 120,000 or more, or 130,000 or more; and 300,000 or less, 250,000 or less, 200,000 or less, 190,000 or less, 180,000 or less, or 170,000 or less.

[0026] Also provided is a method for preparing the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer, which comprises the step of polymerizing a 3-hydroxypropionic acid polymer, lactide and a catalyst.

[0027] The 3-hydroxypropionic acid polymer refers to a homopolymer of 3-hydroxypropionic acid, and a polymer prepared by controlling the degree of polymerization in consideration of the above-mentioned ranges of m and n is used.

[0028] Meanwhile, since the lactide ring-opening polymerization reaction is involved, the preparation method is carried out in the presence of a lactide ring-opening catalyst. For example, the catalyst may be a catalyst represented by Formula 2.

[0029] [Formula 2]

[0030] MA 1 p A 2 2-p

[0031] In formula 2,

[0032] M is Al, Mg, Zn, Ca, Sn, Fe, Y, Sm, Lu, Ti or Zr,

[0033] p is an integer from 0 to 2, and

[0034] A 1 and A 2 Each is independently an alkoxy group or a carboxyl group.

[0035] More specifically, the catalyst represented by Formula 2 may be stannous 2-ethylhexanoate (Sn(OcT)2).

[0036] Preferably, when the total mole number of lactide is considered to be 100 mol %, the catalyst may be used in an amount of 0.001 mol % to 10 mol %, 0.01 mol % to 5 mol % or 0.03 mol % to 1 mol %.

[0037] Preferably, the preparation method is performed at 150° C. to 200° C. Preferably, the preparation method is performed for 5 minutes to 10 hours, and more preferably, for 10 minutes to 1 hour. Preferably, the preparation method is performed at 0.5 atm to 1.5 atm.

[0038] Also provided is a product comprising the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer.

[0039] Beneficial Effects

[0040] As described above, the poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is characterized in that various physical properties of polylactic acid such as tensile strength are improved by introducing monomers derived from 3-hydroxypropionic acid into polylactic acid, thereby expanding its application field. DETAILED DESCRIPTION

[0041] Hereinafter, embodiments of the present invention will be described in more detail in the following examples. However, the following examples are only used to illustrate embodiments of the present invention, and the content of the present invention is not limited by the following examples.

[0042] Preparation Example: Preparation of poly (3-hydroxypropionate) oligomer

[0043] For the biosynthesis of high molecular weight poly (3-hydroxypropionate) according to the present invention, fermentation is first performed under the following conditions to prepare a fermentation broth containing 3-hydroxypropionate as a fermentation substrate. Specifically, Escherichia coli (E. coli) W3110 having GDH and ALDH enzyme genes is used as a fermentation strain. M9 is used as a culture medium, and 70 g / L of glycerol is used as a substrate for fermentation to produce 3-hydroxypropionate.

[0044] Afterwards, the prepared 3-hydroxypropionic acid ester was used as a substrate to produce poly-(3-hydroxypropionic acid) (hereinafter referred to as "P(3HP)") by fermentation. Specifically, a 5L fermentor (internal volume: 3L) was used for fermentation. As a fermentation microorganism, a recombinant Escherichia coli prepared by converting a recombinant vector into XL1-Blue Escherichia coli was used, and the recombinant vector was prepared by cloning the RecC gene as a polyhydroxyalkanoate synthase (PHA synthase) from Ralstonia eutropha and the propionyl-CoA transferase variant 540 (CPPCT_540) gene from Clostridium propionicum into a pBLuescript II KS+ vector.

[0045] The CPPCT_540 gene is an improved gene whose nucleotide sequence is substituted to cause conversion of valine to alanine at position 193 (V194A), and three silent mutations (T669C, A1125G, and T1158C) occur only by DNA substitution without any other amino acid changes (WO09 / 022797).

[0046] As a culture medium, a fermentation broth prepared by adding glucose (20 g / L) and the 3-hydroxypropionate prepared above as substrates to a modified Riesenberg (MR) medium was introduced. This fermentation broth was fermented by aeration at 300 rpm and 1 vvm to finally produce high molecular weight poly (3-hydroxypropionate) (Mn: 136,645; Mw: 354,615; PDI: 2.60; measured using an Agilent 1200 series and calibrated with a PC standard).

[0047] The prepared poly(3-hydroxypropionate) was placed in distilled water and hydrolyzed at 100°C for 18 hours, 24 hours and 72 hours, respectively, to obtain poly(3-hydroxypropionate) oligomers with weight average molecular weights of 30,000 g / mol, 60,000 g / mol and 80,000 g / mol, respectively (measured using Agilent 1200 series and calibrated by PC standards).

[0048] Example 1: Preparation of poly(lactic acid-b-3-hydroxypropionic acid) block copolymer

[0049] Add lactide (25g), poly (3-hydroxypropionate) oligomer (5g) with a weight average molecular weight of 30,000g / mol prepared in the above preparation example, stannous ethylhexanoate (0.014g) and toluene (100uL) as a catalyst into the reactor, and then dry for about 30 minutes to about 1 hour. Then, the reactor is placed in an oil bath preheated to 180°C and polymerized for 1.5 hours. After taking out the product from the reactor, the product is devolatilized at 140°C and 1 to 5 torr under reduced pressure for about 3 hours to remove the monomer. Finally, a poly (lactic acid-b-3-hydroxypropionic acid) block copolymer is prepared.

[0050] Examples 2 to 7: Preparation of poly(lactic acid-b-3-hydroxypropionic acid) block copolymers

[0051] Each poly(lactic acid-b-3-hydroxypropionic acid) block copolymer was prepared in the same manner as in Example 1, except that the starting material was changed as shown in Table 1 below.

[0052] [Table 1]

[0053]

[0054] Comparative Example: Preparation of polylactic acid

[0055] In the reactor, lactide (25g), 1-octanol (0.027g), stannous ethylhexanoate (0.014g) and toluene (100uL) as a catalyst were added, and then dried for about 30 minutes to about 1 hour. Then, the reactor was placed in an oil bath preheated to 180°C and polymerized for 1.5 hours. After the product was taken out from the reactor, the product was devolatilized at 140°C and 1 to 5 torr under reduced pressure for about 3 hours to remove the monomer. Finally, a polylactic acid homopolymer was prepared.

[0056] Test example

[0057] The properties of the copolymers prepared in Examples and Comparative Examples were evaluated as follows.

[0058] - Weight average molecular weight: measured by GPC using Agilent 1200 series and PC standard.

[0059] - Elongation, tensile strength and tensile modulus: performed according to ASTM D638. ASTM D536 V-type specimens were manufactured using a hot press device (Limotem QM900S) and then measured using a universal testing machine (UTM) at a load of 10 mm / s and 60 kg / f.

[0060] - Content of 3-hydroxypropionic acid in the block copolymer (wt%): measured by NMR analysis of the block copolymer.

[0061] The measurement results are shown in Table 2 below.

[0062] [Table 2]

[0063]

Claims

1. A poly (lactic acid-b-3-hydroxypropionic acid) block copolymer represented by the following chemical formula 1, in, The tensile strength of the poly(lactic acid-b-3-hydroxypropionic acid) block copolymer is above 32 MPa: [Chemical formula 1] In Chemical Formula 1, m is an integer from 250 to 650, n is an integer from 600 to 1400, Wherein, m / n is 0.20 to 0.

60.

2. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, wherein m / n is 0.25 to 0.

30.

3. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, wherein The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer has a tensile strength of 60 MPa or less.

4. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, wherein The elongation of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer is 30% to 250%.

5. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, wherein The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer has a tensile modulus of 1.0 GPa to 2.0 GPa.

6. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, wherein The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer has a weight average molecular weight of 50,000 to 350,000.

7. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, wherein The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer has a weight average molecular weight of 130,000 to 170,000.

8. An article comprising the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to any one of claims 1 to 7.