An ultra-thick carbon-based composite coating with a heterogeneous multilayer structure and its preparation method and application
Through the ultra-thick carbon-based composite coating with heterogeneous multi-layer structure, the combination of alternating layered structures and amorphous carbon layers is solved, and the existing carbon-based coatings are insufficient in the marine environment and have low corrosion resistance. It achieves efficient corrosion resistance and long-life performance.
Patent Information
- Application Number
- CN202211572430.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-08
AI Technical Summary
The existing carbon-based coatings are thinner in marine environments due to internal stress, which makes them difficult to serve for a long time. The binding force of traditional single-layer or double-layer structures is low, making it difficult to effectively avoid chloride ions penetration, resulting in insufficient corrosion resistance.
The super-thick carbon-based composite coating with a heterogeneous multi-layer structure is used to form an alternating layered structure through magnetron sputtering technology and ion source-assisted chemical vapor deposition technology, including the heterostructure of MeC layer, MeN layer, and MeCN layer. The outer layer is an amorphous carbon layer, and the outer layer is an amorphous carbon layer, forming a thickness of more than 10 microns to reduce internal stress and enhance density.
It achieves the efficient corrosion resistance and long life of the coating, can effectively block chloride ion penetration, significantly improve the service life of the coating, and provides excellent mechanical and friction wear properties in marine environments.
Smart Images

Figure CN115821206B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material surface protection, and in particular to an ultra-thick carbon-based composite coating with a heterogeneous multilayer structure and a preparation method and application thereof. Background Art
[0002] Due to the high salt, high temperature and high humidity of the marine environment, various metal structures and engineering equipment serving in the marine environment are susceptible to chemical corrosion, electrochemical corrosion, cavitation corrosion and marine biological corrosion. The anti-corrosion of metal materials in the marine environment has always been the focus and research hotspot of researchers, and protecting the surface of materials has become the main means to improve the service life of materials serving in the marine environment.
[0003] Carbon-based coatings prepared by physical vapor deposition methods have attracted a lot of attention due to their excellent tribological properties and chemical inertness. Some people have prepared silicon-doped carbon-based coatings, which have good corrosion resistance due to their dense coating structure to prevent chloride ion attack. Some researchers believe that the dopant changes the passivation behavior of the carbon-based coating by forming inert oxide compounds on the surface, thereby improving the corrosion resistance. However, due to the presence of internal stress during the coating deposition process, the thickness of these coatings is relatively thin, generally around 2 to 5 μm, which makes it difficult for their excellent friction reduction and wear resistance to serve for a long time, and the load-bearing capacity is also greatly restricted. At the same time, the traditional amorphous carbon-based film has a single interface structure, and its single-layer or double-layer structure has a relatively low bonding force. It is difficult to maintain a low wear rate under high shear stress, and the simple single-layer and double-layer structure is difficult to effectively avoid the through pores inside the coating, resulting in chloride ions being able to easily penetrate the coating to contact the substrate, and cannot play a good role in corrosion resistance, thereby greatly reducing the service life of the coating. Ultra-thick coatings are less studied due to the difficulty of preparation and low deposition efficiency. Summary of the invention
[0004] The main purpose of the present invention is to provide an ultra-thick carbon-based composite coating with a heterogeneous multilayer structure and a preparation method and application thereof, so as to overcome the shortcomings of the prior art.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0006] An embodiment of the present invention provides an ultra-thick carbon-based composite coating with a heterogeneous multilayer structure, which includes a transition layer and an alternating layer stacked layer sequentially formed on the surface of a substrate, wherein the alternating layer stacked layer is formed by alternatingly stacking a heterogeneous structure layer and an amorphous carbon layer, and the heterogeneous structure layer includes any one or a combination of more than two of a MeC layer, a MeN layer, and a MeCN layer, and Me is selected from Cr, Ti or W; the outermost layer of the ultra-thick carbon-based composite coating is an amorphous carbon layer.
[0007] The embodiment of the present invention further provides a method for preparing the aforementioned ultra-thick carbon-based composite coating of heterogeneous multilayer structure, which comprises:
[0008] providing a substrate;
[0009] A transition layer is deposited on the surface of the substrate by using magnetron sputtering technology;
[0010] Furthermore, magnetron sputtering technology and ion source assisted chemical vapor deposition technology are used to deposit alternating layers on the surface of the transition layer until an ultra-thick carbon-based composite coating with the heterogeneous multilayer structure is formed.
[0011] The embodiment of the present invention also provides the use of the aforementioned ultra-thick carbon-based composite coating with a heterogeneous multilayer structure in the field of surface protection of metal moving parts in a marine environment.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] (1) The ultra-thick carbon-based composite coating with a heterogeneous multilayer structure provided by the present invention effectively reduces the internal stress of the coating by alternating deposition of heterogeneous structure layers and amorphous carbon layers, so that the coating thickness can reach more than 10 microns. The ultra-thick multilayer structure can effectively avoid through pores inside the coating, effectively blocking chloride ions from penetrating the coating into the substrate, and playing a good role in corrosion resistance, thereby greatly increasing the service life of the coating;
[0014] (2) The ultra-thick carbon-based composite coating with a heterogeneous multilayer structure prepared by the present invention has excellent mechanical properties and friction and wear properties, and also has good corrosion resistance and protection properties, and can be applied to moving parts with long life and corrosion resistance requirements in marine environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0016] Figure 1 Schematic diagram of the structure of an ultra-thick carbon-based composite coating with a heterogeneous multilayer structure in a typical embodiment of the present invention;
[0017] Figure 2 is a SEM image of the cross-sectional structure and morphology of the ultra-thick carbon-based composite coating in Example 1 of the present invention;
[0018] Figure 3 is a long-life friction curve diagram of the ultra-thick carbon-based composite coating in Example 1 of the present invention;
[0019] Figure 4 is a wear morphology curve diagram of the ultra-thick carbon-based composite coating in Example 1 of the present invention after long-life friction;
[0020] Figure 5 This is a macroscopic morphology of the ultra-thick carbon-based composite coating in Example 1 of the present invention after a one-month salt spray test.
[0021] Figure 6 This is a macroscopic photograph of the surface of the coating in Comparative Example 2 of the present invention, which only deposits one heterogeneous structure layer (CrCN layer) and an amorphous carbon layer (DLC layer), after 10 days of salt spray corrosion;
[0022] Figure 7 is a graph showing the friction coefficient of different heterogeneous structure layers in Comparative Example 3 of the present invention;
[0023] Figure 8 It is a scratch adhesion morphology diagram of the coating with a Cr transition layer and the coating without a Cr transition layer in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0024] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] One aspect of an embodiment of the present invention provides an ultra-thick carbon-based composite coating with a heterogeneous multilayer structure, including a transition layer and an alternating layer stacked layer formed in sequence on the surface of a substrate, wherein the alternating layer stacked layer is formed by alternatingly stacking a heterogeneous structure layer and an amorphous carbon layer, the heterogeneous structure layer includes any one or a combination of more than two of a MeC layer, a MeN layer, and a MeCN layer, and Me is selected from Cr, Ti or W; the outermost layer of the ultra-thick carbon-based composite coating is an amorphous carbon layer.
[0026] Specifically, the heterogeneous structure layer in the present invention is mainly some carbide or nitride ceramic phases. These superhard layers of columnar crystal structure can not only provide good support for the amorphous carbon layer, but also effectively block the internal stress accumulated by the amorphous carbon layer, so that the thickness of the entire composite coating can reach more than 10μm. The amorphous carbon layer has a dense structure and can fill the pores of the heterogeneous structure layer of the columnar crystal structure, making the entire coating structure more dense and uniform, and better blocking the role of external moisture and salt, thereby improving the salt spray corrosion performance of the entire coating system and the durability of harsh environments.
[0027] In some more specific embodiments, the structural schematic diagram of the ultra-thick carbon-based composite coating with heterogeneous multilayer structure in the present invention is as follows Figure 1 shown.
[0028] In some more specific embodiments, the ultra-thick carbon-based composite coating has a thickness of more than 10 μm.
[0029] In some more specific embodiments, the thickness of the transition layer is 0.2-1 μm.
[0030] In some more specific embodiments, the thickness of the heterogeneous structure layer is 0.2-1.5 μm.
[0031] In some more specific embodiments, the amorphous carbon layer has a thickness of 0.5 to 3 μm.
[0032] In some more specific embodiments, the alternating stacked layer comprises more than two alternating stacked periodic layers, wherein each alternating stacked periodic layer comprises a heterostructure layer and an amorphous carbon layer.
[0033] In some more specific embodiments, the transition layer includes any one of a Cr layer, a Ti layer, a V layer, and a Mo layer, or a combination of two or more thereof, and is not limited thereto.
[0034] Furthermore, the transition layer is a Cr layer.
[0035] In some more specific embodiments, the Me is selected from Cr.
[0036] In some more specific embodiments, the heterogeneous structure layer includes any one of a CrCN layer, a CrN layer, a CrC layer, and a WC layer, or a combination of two or more thereof, and is not limited thereto.
[0037] In some more specific embodiments, the amorphous carbon layer comprises a diamond-like carbon-based coating.
[0038] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned ultra-thick carbon-based composite coating of heterogeneous multilayer structure, which comprises:
[0039] providing a substrate;
[0040] A transition layer is deposited on the surface of the substrate by using magnetron sputtering technology;
[0041] Furthermore, magnetron sputtering technology and ion source assisted chemical vapor deposition technology are used to deposit alternating layers on the surface of the transition layer until an ultra-thick carbon-based composite coating with the heterogeneous multilayer structure is formed.
[0042] In some more specific embodiments, the preparation method specifically comprises:
[0043] The substrate is placed in a reaction chamber, an inert gas is used as the working atmosphere, a Cr target is used as the target material, and a transition layer is deposited on the surface of the substrate by magnetron sputtering technology, wherein the bias voltage is 0 to -100 V, the target power is 2 to 8 kW, the deposition temperature is 120 to 250° C., the deposition time is 10 to 60 min, and the flow rate of the inert gas is 100 to 300 sccm.
[0044] In some more specific embodiments, the preparation method specifically comprises:
[0045] After the transition layer is deposited, in an inert gas atmosphere, a Cr target is used as a target material, N2 and / or a carbon source gas is used as a working gas, and a magnetron sputtering technology is used to form a heterogeneous structure layer on the surface of the transition layer, wherein the bias voltage is 0 to -100 V, the deposition temperature is 120 to 250° C., the deposition time is 30 to 90 min, the flow rate of N2 is 0 to 1200 sccm, and the flow rate of the carbon source gas is 0 to 300 sccm;
[0046] A graphite target is used as a target material or a carbon source gas is used as a working gas, and magnetron sputtering technology and / or ion source assisted chemical vapor deposition technology are used to deposit an amorphous carbon layer on the surface of the heterogeneous structure layer, wherein the power of the graphite target is 3 to 6 Kw, the deposition temperature is 120 to 250° C., the deposition time is 40 to 120 min, and the flow rate of the carbon source gas is 50 to 500 sccm; when the ion source assisted chemical vapor deposition technology is used, the bias voltage is -600 to -800 V; when the magnetron sputtering technology or the combination of the magnetron sputtering technology and the ion source assisted chemical vapor deposition technology is used, the bias voltage is 0 to -100 V.
[0047] And, the heterogeneous structure layers and the amorphous carbon layers are alternately stacked until the alternately stacked layer is formed.
[0048] Further, the carbon source gas includes C2H2 and / or CH4, but is not limited thereto.
[0049] Furthermore, the heterogeneous structure layer and the amorphous carbon layer are alternately stacked more than twice.
[0050] Further, the inert gas atmosphere includes Ar atmosphere, but is not limited thereto.
[0051] In some specific embodiments, the preparation method further comprises: first evacuating the reaction chamber to a vacuum degree of less than 3×10 -3 Pa, and then the substrate is etched.
[0052] Furthermore, the vacuum is first evacuated to a vacuum better than 3×10 -3Pa, turn on the ion source, heat the filament to 40-60A, introduce protective gas Ar with a flow rate of 30-150sccm, and etch and clean the substrate under a bias voltage of -100V to -400V for 20-60min.
[0053] In some more specific embodiments, the preparation method further includes: The preparation method further includes: pre-treating the surface of the substrate first.
[0054] Furthermore, the pretreatment includes oil and water removal treatment.
[0055] Furthermore, the substrate is first polished and ultrasonically cleaned to remove oil, dust, etc., and then blown dry with dry nitrogen.
[0056] In some more specific embodiments, the material of the substrate includes stainless steel and / or titanium alloy; specifically including stainless steel such as 9Cr18, GCr15, 8Cr4Mo4V, 316, 304, 2Cr13 and titanium alloy substrates such as TC4.
[0057] In some more specific embodiments, the method for preparing the ultra-thick carbon-based composite coating of the heterogeneous multilayer structure specifically includes:
[0058] (1) Using Cr target as target material, applying negative bias voltage to the substrate, and sputtering transition layer on the substrate;
[0059] (2) Using a Cr target or a WC target as a target material, in an Ar gas atmosphere, by introducing N2 and / or C2H2 gas, one or more of WC / CrN / CrC / CrCN are deposited on the transition layer as a heterogeneous structure layer;
[0060] (3) using a graphite target as a target material or C2H2 as a working gas, and using magnetron sputtering technology and / or ion source assisted chemical vapor deposition technology to deposit a diamond-like film on the surface of the heterogeneous structure layer;
[0061] (4) Repeat steps (2) and (3) until the desired coating thickness is reached.
[0062] Another aspect of the embodiments of the present invention further provides the use of the aforementioned ultra-thick carbon-based composite coating with a heterogeneous multilayer structure in the field of surface protection of metal moving parts in harsh environments.
[0063] For example, it is used in the field of surface protection of metal moving parts in marine environments.
[0064] For example, the harsh environment includes high temperature (300-400° C.), high humidity and heat, high salt spray, high speed, high load, high pressure and the like.
[0065] As a preferred solution, the nanocomposite coating is preferably used in the field of friction resistance or corrosion resistance of mechanical parts in marine environments.
[0066] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0067] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0068] Example 1
[0069] In this embodiment, the above-mentioned heterogeneous multilayered ultra-thick carbon-based coating is prepared on the surface of a 316 stainless steel sample, and the specific process steps are as follows:
[0070] (1) Sample pretreatment
[0071] The samples were ultrasonically cleaned in acetone and anhydrous ethanol for more than 15 minutes each, then taken out and blown dry with dry nitrogen;
[0072] (2) Ion etching cleaning
[0073] The sample treated in step (1) was placed in a magnetron sputtering chamber and evacuated to a vacuum better than 3×10 -3 Pa; turn on the ion source, heat the filament to 40A, introduce 60sccm of high-purity argon, apply a negative bias to the substrate, and etch and clean the substrate at a bias of -200V to remove impurities such as dust attached to the surface. The etching time is 30min;
[0074] (3) Deposition of Cr transition layer
[0075] Use metal Cr as the target (purity ≥ 99.9%), open the Cr target to sputter the transition layer after ion etching, control the Ar gas flow rate to 150sccm, the bias voltage to -50V, the target power to 6Kw, the sputtering time to 30min, and the thickness to 0.5μm;
[0076] (4) Deposition of CrCN layer
[0077] The C2H2 flow rate was controlled to be 100 sccm, the Ar gas flow rate was 0 sccm, the N2 gas flow rate was 1000 sccm, the bias voltage and the Cr target power were kept constant, the sputtering time was 60 min, and the CrCN coating thickness was about 1.4 μm;
[0078] (5) Deposition of DLC layer
[0079] The Cr target power was gradually reduced to 0, the N2 gas flow was gradually reduced to 0, the C2H2 flow was increased to 300 sccm, the turntable bias was increased to -650 V, and the DLC coating was formed by ionizing the C2H2 gas at a high bias voltage. The deposition time was 60 min and the coating thickness was 2.3 μm.
[0080] (6) Deposition of multilayer structures
[0081] Steps (4) and (5) were repeated 4 times to form an ultra-thick carbon-based composite coating with a heterogeneous multilayer structure, with a total coating thickness of about 15 μm. After the coating was completed, the coating was cooled to room temperature in the furnace and then re-pressed and taken out. Figure 2 This is the cross-sectional morphology of the ultra-thick carbon-based coating with a heterogeneous multilayer structure in Example 1 of the present invention.
[0082] The CSM friction and wear tester was used to test and evaluate the long-life friction and wear performance of the coating. The specific method is: a rotating friction test is performed on the coating sample and the friction pair, with a rotation radius of 10mm, a load of 5N, and a friction pair of The 9Cr18 steel ball was tested for 800,000 revolutions. The curve of friction coefficient changing with revolutions is as follows Figure 3 As shown in the figure, the friction coefficient was about 0.06 before 600,000 revolutions, and then gradually increased to 0.13. The wear profile after friction is as follows Figure 4 As shown in the figure, the wear scar depth is about 1.5 μm, and the calculated wear rate is 8.9×10 -7 mm 3 / Nm. The coated sample was placed in a circulating salt spray corrosion device for a neutral salt spray corrosion test. The environment was a 5% NaCl solution at a temperature of 35°C. The macroscopic state of the sample surface after the test was Figure 5 The results show that the coating sample has excellent long-life friction and wear performance, and no rust spots appear after a 1-month salt spray test, and has good corrosion resistance.
[0083] Example 2
[0084] In this embodiment, the above-mentioned heterogeneous multilayered ultra-thick carbon-based coating is prepared on the surface of 8Cr4Mo4V bearing steel, and the specific process steps are as follows:
[0085] (1) Sample pretreatment is the same as in Example 1;
[0086] (2) Ion etching cleaning
[0087] The sample treated in step (1) was placed in a magnetron sputtering chamber and evacuated to a vacuum better than 3×10 -3Pa; turn on the ion source, heat the filament to 50A, introduce 80sccm of high-purity argon, apply a negative bias to the substrate, and etch and clean the substrate at a bias of -200V to remove impurities such as dust attached to the surface. The etching time is 20min;
[0088] (3) Deposition of Cr transition layer
[0089] Use metal Cr as the target (purity ≥ 99.9%), open the Cr target to sputter the transition layer after ion etching, control the Ar gas flow rate to 100sccm, the bias voltage to -100V, the target power to 4Kw, the sputtering time to 40min, and the thickness to about 0.6μm;
[0090] (4) Deposition of CrN layer
[0091] The Ar gas flow rate was controlled to be 0, the N2 gas flow rate was controlled to be 800 sccm, the bias voltage and the Cr target power were kept constant, the sputtering time was 50 min, and the thickness of the CrN layer was about 1.0 μm;
[0092] (5) Deposition of DLC layer
[0093] Gradually reduce the Cr target power to 0, gradually reduce the N2 gas flow to 0, increase the C2H2 flow to 280sccm, increase the turntable bias to -600V, and form the DLC coating by ionizing the C2H2 gas with high bias. The deposition time is 50min and the coating thickness is about 1.8μm.
[0094] (6) Deposition of multilayer structures
[0095] The processes (4) and (5) were repeated 8 times to form an ultra-thick carbon-based composite coating with a heterogeneous multilayer structure, with a total coating thickness of about 23 μm. After the coating was completed, the coating was cooled to room temperature in the furnace and then re-pressed and taken out.
[0096] Example 3
[0097] In this embodiment, the above-mentioned heterogeneous multilayered ultra-thick carbon-based coating is prepared on the surface of TC4 titanium alloy, and the specific process steps are as follows:
[0098] (1) Sample pretreatment is the same as in Example 1;
[0099] (2) Ion etching cleaning
[0100] The sample treated in step (1) was placed in a magnetron sputtering chamber and evacuated to a vacuum better than 3×10 -3 Pa; turn on the ion source, heat the filament to 60A, introduce 150sccm of high-purity argon, apply a negative bias to the substrate, and etch and clean the substrate at a bias of -300V to remove impurities such as dust attached to the surface. The etching time is 40min;
[0101] (3) Deposition of Cr transition layer
[0102] Use metal Cr as the target (purity ≥ 99.9%), open the Cr target to sputter the transition layer after ion etching, control the Ar gas flow rate to 150sccm, the bias voltage to 0V, the target power to 8Kw, the sputtering time to 15min, and the thickness to about 0.8μm;
[0103] (4) Deposition of CrC layer
[0104] The C2H2 flow rate was controlled to be 200sccm, the Ar gas flow rate was 300sccm, the bias voltage and the Cr target power were kept constant, the sputtering time was 30min, and the CrC layer thickness was about 0.8μm;
[0105] (5) Deposition of DLC layer
[0106] The Cr target power was gradually reduced to 0, while the C2H2 flow rate was increased to 450sccm, the turret bias was increased to -800V, and the DLC coating was formed by ionizing the C2H2 gas at a high bias voltage. The deposition time was 40min and the coating thickness was 1.4μm.
[0107] (6) Deposition of multilayer structures
[0108] The processes (4) and (5) were repeated 10 times to form an ultra-thick carbon-based composite coating with a heterogeneous multilayer structure, with a total coating thickness of about 22 μm. After the coating was completed, the coating was cooled to room temperature in the furnace and then re-pressed and taken out.
[0109] Example 4
[0110] In this embodiment, the above-mentioned heterogeneous multilayered ultra-thick carbon-based coating is prepared on the surface of TC4 titanium alloy, and the specific process steps are as follows:
[0111] (1) Sample pretreatment is the same as in Example 1;
[0112] (2) Ion etching cleaning
[0113] The sample treated in step (1) was placed in a magnetron sputtering chamber and evacuated to a vacuum better than 3×10 -3 Pa; turn on the ion source, heat the filament to 60A, introduce 30sccm of high-purity argon, apply a negative bias to the substrate, and etch and clean the substrate at a bias of -400V to remove impurities such as dust attached to the surface. The etching time is 60min;
[0114] (3) Deposition of Ti transition layer
[0115] Use metal Ti as the target (purity ≥ 99.9%), open the Ti target to sputter the transition layer after ion etching, control the Ar gas flow rate to 150sccm, the bias voltage to -50V, the target power to 2Kw, the sputtering time to 60min, and the thickness to about 0.3μm;
[0116] (4) Deposition of WC layer
[0117] Control the C2H2 flow rate to 50sccm, the Ar gas flow rate to 200sccm, the WC target (purity ≥ 99.9%) power to 4Kw, the bias voltage to -100V, the sputtering time to 90min, and the WC layer thickness to about 1.5μm;
[0118] (5) Deposition of DLC layer
[0119] Gradually reduce the WC target power to 0, increase the graphite target (purity ≥ 99.9%) power to 5Kw, and increase the C2H2 flow rate to 80sccm. Keep the turntable bias at -100V, and form the DLC coating through the combined action of magnetron sputtering graphite target and ionized C2H2 gas. The deposition time is 60min and the coating thickness is 2.8μm.
[0120] (6) Deposition of multilayer structures
[0121] The processes (4) and (5) were repeated 6 times to form an ultra-thick carbon-based composite coating with a heterogeneous multilayer structure, and the total thickness of the coating was about 26 μm. After the coating was completed, the coating was cooled to room temperature in the furnace and then re-pressed and taken out.
[0122] Comparative Example 1
[0123] The method is the same as Example 1, except that no heterogeneous structure layer (CrCN layer) is deposited; since the prepared coating has no heterogeneous structure layer, the single amorphous carbon layer has excessive internal stress due to continuous accumulation of stress, and the coating generally peels off after a thickness of 5 to 6 μm.
[0124] Comparative Example 2
[0125] The method is the same as that of Example 1, except that only one layer of heterogeneous structure layer (CrCN layer) and amorphous carbon layer (DLC layer) are deposited; the coating with only one layer of heterogeneous structure layer and amorphous carbon layer will still wear out and fail under the long-term friction and wear conditions of the moving parts due to its limited thickness (about 2-5 μm), and cannot work for a long time. Moreover, the limited thickness cannot play a good role in Cl -1 The isolation effect of the coating is poor, so the salt spray corrosion performance is poor, and it cannot achieve the application effect of long-life operation in harsh environments. The surface macroscopic photo of the coating with only one layer of heterogeneous structure layer (CrCN layer) and amorphous carbon layer (DLC layer) after 10 days of salt spray corrosion is shown in the figure below. Figure 6 As shown, it can be seen from the figure that obvious corrosion pits have appeared in the figure.
[0126] Comparative Example 3
[0127] The method is the same as the above-mentioned Example 1, except that no amorphous carbon layer (DLC layer) is deposited; the friction coefficient of the coating with only a heterogeneous structure layer without amorphous carbon layer is generally between 0.3 and 0.7, which does not have the effect of reducing friction, and these heterogeneous structure layers are basically columnar crystal structures with many physical pores, which makes the corrosion resistance of the coating poor and cannot meet the use in salt spray corrosion environment. The friction coefficient curves of different heterogeneous structure layers are as follows: Figure 7 shown.
[0128] Comparative Example 4
[0129] The method is the same as Example 1, except that no Cr transition layer is deposited. The transition layer mainly serves as a connection transition between the substrate and the coating. The coating without the transition layer has poor bonding strength with the substrate and is very easy to peel off during the movement of the parts. The hard particles formed after peeling further aggravate the wear of the moving parts. The coating not only fails to play the due protective role, but also accelerates the failure of the moving parts. The scratch bonding strength of the coating with the transition layer and the coating without the Cr transition layer is as follows: Figure 8 shown.
[0130] In summary, the ultra-thick carbon-based composite coating with a heterogeneous multilayer structure provided by the present invention can quickly prepare an ultra-thick carbon-based coating through the design of a heterogeneous multilayer structure, and the coating has long-term excellent tribological properties and good corrosion resistance.
[0131] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0132] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. An ultra-thick carbon-based composite coating with a heterogeneous multilayer structure, characterized in that The invention comprises a transition layer and an alternating layer stacked layer sequentially formed on the surface of a substrate, wherein the alternating layer stacked layer is formed by alternating heterogeneous structure layers and amorphous carbon layers, the heterogeneous structure layers include MeCN layers, and Me is selected from Cr, Ti or W; the outermost layer of the ultra-thick carbon-based composite coating is an amorphous carbon layer; the thickness of the ultra-thick carbon-based composite coating is more than 10 μm; the amorphous carbon layer is a diamond-like carbon-based coating; The thickness of the transition layer is 0.5-1 μm; the thickness of the heterogeneous structure layer is 1.4-1.5 μm; the thickness of the amorphous carbon layer is 2.3-3 μm; the alternating stacking layer comprises more than two alternating stacking periodic layers, wherein each alternating stacking periodic layer comprises a heterogeneous structure layer and an amorphous carbon layer; The method for preparing the ultra-thick carbon-based composite coating of the heterogeneous multilayer structure comprises: providing a substrate; The substrate is placed in a reaction chamber, an inert gas is used as the working atmosphere, a Cr target is used as the target material, and a transition layer is deposited on the surface of the substrate by magnetron sputtering technology, wherein the bias voltage is 0-100V, the target power is 2-8kw, the deposition temperature is 120-250°C, the deposition time is 10-60min, and the flow rate of the inert gas is 100-300sccm; After the transition layer is deposited, in an inert gas atmosphere, a Cr target is used as a target material, N2 and a carbon source gas are used as working gases, and a magnetron sputtering technology is used to form a heterogeneous structure layer on the surface of the transition layer, wherein the bias voltage is 0~-100V, the deposition temperature is 120~250°C, the deposition time is 30~90min, the flow rate of N2 is 0~1200sccm, and the flow rate of the carbon source gas is 0~300sccm; Using carbon source gas as working gas, an ion source assisted chemical vapor deposition technique is used to deposit an amorphous carbon layer on the surface of the heterogeneous structure layer, wherein the deposition temperature is 120-250° C., the deposition time is 40-120 min, the flow rate of the carbon source gas is 50-500 sccm, and the bias voltage is -600--800 V; And, the heterogeneous structure layer and the amorphous carbon layer are alternately stacked until the alternately stacked layer is formed, thereby forming the ultra-thick carbon-based composite coating of the heterogeneous multilayer structure.
2. The ultra-thick carbon-based composite coating according to claim 1, characterized in that: The transition layer is selected from any one of a Cr layer, a Ti layer, a V layer, and a Mo layer, or a combination of two or more thereof.
3. The ultra-thick carbon-based composite coating according to claim 2, characterized in that: The transition layer is a Cr layer.
4. The ultra-thick carbon-based composite coating according to claim 1, characterized in that: The Me is Cr.
5. The ultra-thick carbon-based composite coating of heterogeneous multilayer structure according to claim 1, characterized in that: The carbon source gas is selected from C2H2 and / or CH4.
6. The ultra-thick carbon-based composite coating of heterogeneous multilayer structure according to claim 1, characterized in that: The heterogeneous structure layer and the amorphous carbon layer are alternately stacked more than twice.
7. The ultra-thick carbon-based composite coating of heterogeneous multilayer structure according to claim 1, characterized in that: The inert gas atmosphere is Ar atmosphere.
8. The ultra-thick carbon-based composite coating of heterogeneous multilayer structure according to claim 1, characterized in that: The method for preparing the ultra-thick carbon-based composite coating of the heterogeneous multilayer structure further comprises: firstly evacuating the reaction chamber to a vacuum degree of less than 3×10 - 3 Pa, and then the substrate is etched.
9. The ultra-thick carbon-based composite coating of heterogeneous multilayer structure according to claim 1, characterized in that: The method for preparing the ultra-thick carbon-based composite coating with a heterogeneous multilayer structure also includes: firstly pre-treating the surface of the substrate; the pre-treatment includes degreasing and dewatering treatment.
10. The ultra-thick carbon-based composite coating of heterogeneous multilayer structure according to claim 1, characterized in that: The material of the substrate is selected from stainless steel and / or titanium alloy.
11. Use of the ultra-thick carbon-based composite coating of any one of claims 1 to 10 in the field of surface protection of metal moving parts in harsh environments.