A high temperature resistant and anti-oxidation absorbing film and a preparation method thereof
By depositing a silicon carbide coating on the absorbing film, the oxidation resistance of the carbon fiber is improved, which solves the problem of rapid oxidation rate of the traditional absorbing film at high temperatures and achieves higher oxidation temperature and anti-oxidation performance.
Patent Information
- Application Number
- CN202211664810.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The absorbing electromagnetic film obtained by doping traditional chopped carbon fiber with low-dielectric chopped fiber has a fast oxidation rate at high temperatures and insufficient oxidation resistance. It cannot meet the temperature resistance requirements of the new generation of high-speed aircraft.
By mixing chopped carbon fibers with low-dielectric chopped fibers, a fiber mesh is made, and the fiber mesh is coated with glue, dried, and then impregnated with polycarbosilane for high-temperature cracking to deposit a silicon carbide coating to improve the oxidation resistance of the carbon fiber.
The oxidation temperature of the absorbing film is significantly increased from the original 480°C to 575°C, 580°C or 585°C, which enhances the oxidation resistance of the carbon fiber and meets the demand for high-temperature absorbing materials.
Smart Images

Figure CN115821576B_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a high temperature resistant and anti-oxidation wave absorbing film and a preparation method thereof, belonging to the technical field of functional materials. Background Art
[0002] High-temperature absorbing materials have important application value in the field of new generation military equipment because they have the functions of high temperature resistance and electromagnetic wave absorption, and therefore have received extensive attention. Traditional high-temperature absorbing materials are usually prepared by a certain composite process using high-temperature resistant absorbents and ceramic or glass matrices. Current research mainly focuses on adjusting the electromagnetic parameters, mixing performance and other physical and chemical properties of the absorbent through the doping, modification, morphology control and distribution state of the high-temperature absorbent in the matrix, so as to adjust the equivalent electromagnetic matching performance, mechanical properties, high temperature resistance and other properties of the high-temperature absorbing material. Electromagnetic film is a technical approach to adjust the electromagnetic parameters of the absorbent by dispersing the absorbent in the matrix and then adjusting the distribution state of the absorbent in the matrix. Carbon fiber has high strength, high modulus and good electrical conductivity. It is a key fiber commonly used in structural absorbing materials that has both reinforcement characteristics and electromagnetic loss characteristics. It plays an important role in structural stealth materials. The chopped carbon fiber electromagnetic absorbing film obtained by mixing chopped carbon fiber with low dielectric chopped fiber plays an important role in the preparation of structural absorbing materials.
[0003] With the development of a new generation of high-speed aircraft, equipment has also put forward higher requirements for the temperature resistance of materials. For example, during the flight of a supersonic cruise aircraft, due to aerodynamic heating, the thermal equilibrium temperature of the outer surface of the structure reaches above 600°C. Test data show that the oxidation rate of carbon fiber increases significantly at about 500°C, the antioxidant capacity decreases sharply, and the weight loss rate is as high as more than 50%, which seriously affects the application of materials and components. As a result, the chopped carbon fiber absorbing electromagnetic film obtained by doping chopped carbon fiber with low dielectric chopped fiber loses its function. Therefore, it is necessary to improve the antioxidant capacity of chopped carbon fiber doped with low dielectric chopped fiber absorbing electromagnetic film to provide technical support for the development of high-temperature absorbing structural materials.
[0004] In the existing preparation technology of hybrid chopped carbon fiber electromagnetic film, the technical solution provided by patent document CN102206371A is to mix chopped carbon fiber with recycled rubber, and then mix them evenly on an open mixer and an internal mixer, and press them into thin sheets to obtain the product. Since this technology does not add low-dielectric chopped fibers, but only chopped carbon fibers with strong conductivity, a rubber-based high-reflection electromagnetic shielding film is prepared. The main function of the product is to serve as a reflective layer of a structural absorbing material. The material thickness is relatively large (0.5-15mm), and the temperature resistance is lower than 300°C, which cannot meet the requirement of greater than 600°C required by the technical background. Summary of the invention
[0005] The purpose of the present invention is to provide a high temperature resistant and anti-oxidation absorbing film and a preparation method thereof, which can effectively improve the anti-oxidation ability of carbon fiber as an electrical loss absorber. The absorbing film is coated with a SiC anti-oxidation layer by impregnating polycarbosilane and high temperature cracking, which greatly improves the high temperature resistance of the carbon fiber conductive absorber.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a high temperature resistant and anti-oxidation absorbing film comprises the following steps:
[0008] 1) Chopped carbon fibers and low-dielectric chopped fibers are selected, wherein the low-dielectric chopped fibers are one or more of glass chopped fibers, quartz chopped fibers, and alumina chopped fibers;
[0009] 2) mixing the chopped carbon fibers and the low dielectric chopped fibers selected in step 1), adding water and a dispersant and mixing them evenly;
[0010] 3) the mixed fiber obtained in step 2) is made into a fiber web by using a papermaking process;
[0011] 4) applying glue to the fiber web obtained in step 3);
[0012] 5) placing the fiber web coated with the glue obtained in step 4) on a press to pressurize and squeeze out excess glue;
[0013] 6) drying the glue solution to obtain a dried absorbing film;
[0014] 7) The dried absorbing film is immersed in polycarbosilane for high-temperature cracking, and a silicon carbide coating is deposited on the absorbing film to obtain a high-temperature resistant and anti-oxidation absorbing film.
[0015] Furthermore, the chopped carbon fiber may be one or more of chopped T300 carbon fiber, chopped T700 carbon fiber, chopped T800 carbon fiber, chopped T1000 carbon fiber, chopped M300J carbon fiber, and chopped M550J carbon fiber.
[0016] Furthermore, when the two materials are mixed in step 2), the mass proportion of the chopped carbon fibers is 0.05% to 15%.
[0017] Furthermore, in step 2), the mass of the water is 15 to 35 times the mass of the two fiber mixtures, and the mass of the dispersant is 0.018% to 0.06% of the mass of the water.
[0018] Furthermore, the glue applied in step 4) is one of epoxy resin glue, bismaleimide glue, polyvinyl alcohol.
[0019] Furthermore, in step 6), the drying temperature of the glue solution is 105±5° C., and the drying time is 5 to 10 minutes.
[0020] Furthermore, in step 7), the dried absorbing film is immersed in polycarbosilane for 2 to 8 hours, then taken out and placed in a muffle furnace, the muffle furnace is heated to 200 to 400°C at a rate of 5 to 10°C / min, and cured at this temperature for 2 to 6 hours; then the muffle furnace is further heated to 900 to 1100°C, and the polycarbosilane is pyrolyzed at high temperature for 2 to 4 hours.
[0021] A high temperature resistant and anti-oxidation wave absorbing film is prepared by the above preparation method.
[0022] The present invention provides a high temperature resistant and anti-oxidation absorbing film, which is based on a chopped carbon fiber and a low dielectric chopped fiber mixed absorbing film, by fully impregnating the prepared absorbing film in polycarbosilane, and then pyrolyzing the polycarbosilane at high temperature in a muffle furnace, so that an anti-oxidation silicon carbide coating is deposited on the surface of the prepared absorbing film. The absorbing film (thickness of 0.1 to 0.3 mm) obtained in this way can effectively improve the anti-oxidation ability of carbon fiber while maintaining the good dielectric properties of carbon fiber as an absorbent, thereby realizing the high temperature strong absorption function of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic structural diagram of a high temperature resistant and anti-oxidation absorbing film proposed by the present invention.
[0024] Figure 2 This is a photo of the high temperature resistant and anti-oxidation absorbing film sample prepared in Example 1. DETAILED DESCRIPTION
[0025] In order to make the above features and advantages of the present invention more obvious and easy to understand, embodiments are given below and described in detail with reference to the accompanying drawings.
[0026] Example 1
[0027] Step 1: Weigh 0.06g of chopped T300 carbon fiber and 119.8g of glass fiber.
[0028] Step 2: Add 2 kg of water and 0.36 g of dispersant methyl acrylate to the two fiber mixture and mix well.
[0029] Step 3: Filter the liquid of the mixed slurry by suction, and form the mixed fiber into a web by using a papermaking process;
[0030] Step 4: Weigh a total of 36 g of adhesive PVA and apply it evenly on the obtained mixed fiber web;
[0031] Step 5: placing the film coated with the glue on a press to pressurize and squeeze out excess glue;
[0032] Step 6: Raise the temperature of the flat press to 110°C and keep it warm for 5 minutes to dry the glue solution;
[0033] Step 7: Immerse the dried absorbing film in polycarbosilane for 2 hours, then take it out and place it in a muffle furnace, heat it to 200°C and cure it for 6 hours, then continue to heat it to 900°C and perform high-temperature pyrolysis for 4 hours to obtain a high-temperature resistant and anti-oxidation absorbing film.
[0034] Product performance test: The prepared absorbing film is as above Figure 2 As shown, the oxidation temperature was increased from 480°C to 575°C after testing.
[0035] Example 2
[0036] Step 1: Weigh 28.1 g of silicon carbide coated chopped T300 carbon fiber and 159.2 g of glass fiber.
[0037] Step 2: Add 4 kg of water and 1.6 g of dispersant methyl acrylate to the two fiber mixture and mix well.
[0038] Step 3: Filter the liquid of the mixed slurry by suction, and form the mixed fiber into a web by using a papermaking process;
[0039] Step 4: Weigh a total of 6.4 g of adhesive PVA and apply it evenly on the obtained mixed fiber web;
[0040] Step 5: placing the film coated with the glue on a press to pressurize and squeeze out excess glue;
[0041] Step 6: Raise the temperature of the flat press to 105° C., keep the temperature for 8 minutes, and dry the glue solution to obtain the high temperature resistant and anti-oxidation absorbing film of the present invention.
[0042] Step 7: Immerse the dried absorbing film in polycarbosilane for 4 hours, then take it out and place it in a muffle furnace, heat it to 280°C for curing for 3 hours, then continue to heat it to 1050°C and perform high-temperature pyrolysis for 3 hours to obtain a high-temperature resistant and anti-oxidation absorbing film.
[0043] Product performance test: The oxidation temperature of the prepared absorbing film was increased from the original 480℃ to 580℃.
[0044] Example 3
[0045] Step 1: Weigh 1.8 g of silicon carbide coated chopped T300 carbon fiber and 298.2 g of glass fiber.
[0046] Step 2: Add 10 kg of water and 6 g of dispersant methyl acrylate to the two fiber mixture and mix well.
[0047] Step 3: Filter the liquid of the mixed slurry by suction, and form the mixed fiber into a web by using a papermaking process;
[0048] Step 4: Weigh a total of 9 g of adhesive PVA and evenly apply it on the obtained mixed fiber web;
[0049] Step 5: placing the film coated with the glue on a press to pressurize and squeeze out excess glue;
[0050] Step 6: Raise the temperature of the flat press to 100° C., keep it warm for 10 minutes, and dry the glue solution to obtain the high temperature resistant and anti-oxidation absorbing film of the present invention.
[0051] Step 7: Immerse the dried absorbing film in polycarbosilane for 8 hours, then take it out and place it in a muffle furnace, heat it to 400°C and cure it for 2 hours, then continue to heat it to 1100°C and perform high-temperature pyrolysis for 2 hours to obtain a high-temperature resistant and anti-oxidation absorbing film.
[0052] Product performance test: The oxidation temperature of the prepared absorbing film was increased from the original 480℃ to 585℃.
[0053] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the present invention. Appropriate modifications or equivalent substitutions of the technical solutions of the present invention made by ordinary technicians in the field should all be included in the protection scope of the present invention. The protection scope of the present invention shall be based on what is defined in the claims.
Claims
1. A method for preparing a high temperature resistant and anti-oxidation absorbing film, characterized in that: The following steps are involved: 1) Chopped carbon fibers and low-dielectric chopped fibers are selected, wherein the low-dielectric chopped fibers are one or more of glass chopped fibers, quartz chopped fibers, and alumina chopped fibers; 2) mixing the chopped carbon fibers and the low dielectric chopped fibers selected in step 1), adding water and a dispersant and mixing them evenly; 3) the mixed fiber obtained in step 2) is made into a fiber web by using a papermaking process; 4) applying glue to the fiber web obtained in step 3); 5) placing the fiber web coated with the glue obtained in step 4) on a press to pressurize and squeeze out excess glue; 6) drying the glue solution to obtain a dried absorbing film; 7) The dried absorbing film is immersed in polycarbosilane for 2 to 8 hours, then taken out and placed in a muffle furnace, the muffle furnace is heated to 200 to 400° C., and the film is cured at this temperature for 2 to 6 hours; then the muffle furnace is further heated to 900 to 1100° C., the polycarbosilane is pyrolyzed at high temperature for 2 to 4 hours, and a silicon carbide coating is deposited on the absorbing film, thereby obtaining a high temperature resistant and anti-oxidation absorbing film.
2. The preparation method according to claim 1, characterized in that The chopped carbon fiber may be one or more of chopped T300 carbon fiber, chopped T700 carbon fiber, chopped T800 carbon fiber, chopped T1000 carbon fiber, chopped M300J carbon fiber and chopped M550J carbon fiber.
3. The preparation method according to claim 1, characterized in that: When the two are mixed in step 2), the mass proportion of the chopped carbon fibers is 0.05% to 15%.
4. The preparation method according to claim 1, characterized in that: In step 2), the mass of the water is 15 to 35 times the mass of the two fiber mixtures, and the mass of the dispersant is 0.018% to 0.06% of the mass of the water.
5. The preparation method according to claim 1, characterized in that: The glue applied in step 4) is one of epoxy resin glue, bismaleimide glue, polyvinyl alcohol.
6. The preparation method according to claim 1, characterized in that: In step 6), the glue solution is dried at a temperature of 105±5° C. for 5 to 10 minutes.
7. A high temperature resistant and anti-oxidation absorbing film, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Reclaimed rubber composite material with electromagnetic shielding performance and preparation method thereof
CN102206371A
Method for preparing carbon-fiber-reinforced silicon carbide composite material
CN102249721A
High-temperature resin-based structure wave-absorbing composite material and preparation method thereof
CN114055866A