A three-dimensional ordered macroporous high-entropy perovskite monolithic catalytic device and its preparation method and application
The three-dimensional ordered large-pore high-entropy perovskite catalytic devices are prepared by one-step method, which solves the problem of low contact efficiency of high-entropy materials, significantly improves catalytic activity and stability, and is suitable for diesel vehicle exhaust, VOCs and coal mine gas methane Catalytic combustion purification.
Patent Information
- Application Number
- CN202211461354.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-17
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-17
AI Technical Summary
The existing high-entropy material catalysts have the problem of low catalyst contact efficiency and need to improve catalytic activity.
A one-step method is used to prepare a three-dimensional ordered macroporous high entropy perovskite integral catalytic device. By dissolving salt containing A and B elements, adding organic acids and polystyrene microsphere dispersion, immersing them on a honeycomb ceramic matrix and then calcining them. , form high-entropy perovskite oxides, and improve the mass transfer and diffusion performance of catalytic devices.
The three-dimensional ordered macropore structure generation of catalytic devices is realized, which improves catalytic activity and stability, has good high temperature, humidity and sulfur resistance, and significantly improves catalytic combustion activity.
Smart Images

Figure CN115845868B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of environmental catalysis technology, and in particular to a three-dimensional ordered macroporous high-entropy perovskite monolithic catalytic device and a preparation method and application thereof. Background Art
[0002] The development of new catalytic materials may bring breakthroughs and revolutionary changes to the field of environmental catalytic technology, and help environmental catalysis (such as catalytic purification of diesel vehicle carbon soot particles, catalytic purification of coal mine gas methane, and catalytic combustion of industrial VOCs), which has important economic, environmental and social significance. High entropy materials have developed rapidly in recent years. With their unique structure, they have shown excellent performance in many fields and are increasingly widely used. High entropy materials refer to materials composed of at least five or more chemical elements in equal or nearly equal molar ratios. High entropy perovskites are high entropy perovskite structures formed by multiple cations occupying different positions in the lattice under the concept of high entropy. High entropy materials have four major characteristics: thermodynamic high entropy effect, lattice distortion effect, dynamic hysteresis diffusion effect, and cocktail effect. Among them, due to the large number of elements in high entropy materials, the differences in atomic radius and binding energy are more significant than those in traditional materials, so they show more significant lattice distortion than traditional materials, which makes them have dynamic hysteresis diffusion phenomenon and anti-grain coarsening behavior. Therefore, high entropy materials show higher stability than traditional materials when used as catalysts, and are more suitable for the field of high-temperature thermal catalysis. However, current high-entropy material catalysts generally suffer from the problem of low catalyst contact efficiency, and their catalytic activity needs to be further improved. Summary of the invention
[0003] The purpose of the present invention is to provide a three-dimensional ordered macroporous high-entropy perovskite monolithic catalytic device and its preparation method and application, so as to solve the problems existing in the above-mentioned prior art. A simple "one-step" preparation process is used to prepare the high-entropy perovskite monolithic catalytic device into a three-dimensional ordered macroporous structure, thereby improving the mass transfer and diffusion performance of the catalytic device and thus improving its catalytic activity.
[0004] To achieve the above object, the present invention provides the following solutions:
[0005] One of the technical solutions of the present invention is a high entropy perovskite monolithic catalytic device, wherein the high entropy perovskite monolithic catalytic device comprises a substrate and a high entropy perovskite oxide;
[0006] The high entropy perovskite oxide is loaded on the surface of the substrate;
[0007] The high entropy perovskite oxide has a three-dimensional ordered macroporous structure;
[0008] The chemical formula of the high entropy perovskite oxide is ABO 3, wherein the A element is selected from one or more of Ca, K, La, Sr, Bi, Gd, Nd, Sm, and Y; the B element is selected from one or more of Cr, Mn, Fe, Co, Ni, Cu, Ti, and Al; and at least one of the A element and the B element is composed of five or more elements in equal molar ratios.
[0009] Furthermore, the loading amount of the entropic perovskite oxide catalyst is 1-20wt%.
[0010] Further, the substrate is a ceramic substrate or a metal alloy substrate with a honeycomb structure, the substrate is a cylinder, a cuboid or a cube; the diameter of the cylinder is 5-100 cm, the height is 2-100 cm, the length and width of the cuboid or cube are 5-100 cm, respectively, and the height is 2-100 cm; the pore size of the three-dimensional ordered macroporous structure is 0.5 μm-2 μm, and the porosity is 1-20%. Preferably, the substrate is a ceramic substrate.
[0011] The second technical solution of the present invention is a method for preparing the above-mentioned high entropy perovskite monolithic catalytic device, comprising the following steps:
[0012] A salt containing element A and a salt containing element B are added into water to dissolve, and then an organic acid and an organic solvent are added to obtain a mixed metal salt sol;
[0013] adding a polystyrene microsphere dispersion to the mixed metal salt sol to obtain a mixed dispersion;
[0014] The substrate is immersed in the mixed dispersion, and after the immersion is completed, it is dried and calcined to obtain the high entropy perovskite monolithic catalytic device.
[0015] Furthermore, the concentration of the mixed metal salt sol is 0.2 mol / L-2.2 mol / L.
[0016] Furthermore, the salt containing element A is a nitrate of element A; the salt containing element B is a nitrate of element B; the organic acid is oxalic acid, citric acid or fruit acid; the organic solvent is ethylene glycol; and the polystyrene microsphere dispersion is a polystyrene microsphere ethylene glycol dispersion.
[0017] Furthermore, the concentration of the polystyrene microsphere dispersion is 10 g / L; and the ratio of the total mass of the salt containing element A and the salt containing element B to the mass of the polystyrene microspheres is 5:1.
[0018] Furthermore, the impregnation time is 5-20 hours; the drying is specifically 10-30 hours at 50°C; and the calcination is specifically 20-30 hours at 800°C. The drying and calcination time are conducive to the formation of a three-dimensional ordered macroporous structure and the formation of a single-phase high-entropy perovskite, so that it does not separate into phases, and can effectively improve the high temperature resistance and mass transfer and diffusion performance of the catalytic material. Higher or lower than the above-mentioned range will affect the formation of a three-dimensional ordered macroporous structure and a single-phase high-entropy perovskite.
[0019] The third technical solution of the present invention is the application of the above-mentioned high entropy perovskite monolithic catalytic device in a diesel vehicle exhaust particulate matter collector.
[0020] A fourth technical solution of the present invention is the application of the above-mentioned high entropy perovskite monolithic catalytic device in the catalytic combustion purification of VOCs in coal chemical industry, wherein the temperature of the catalytic combustion purification is 150-400°C.
[0021] A fifth technical solution of the present invention is the application of the above-mentioned high entropy perovskite monolithic catalytic device in the catalytic combustion purification of methane in coal mine ventilation gas, and the temperature of the catalytic combustion purification is 350-600°C.
[0022] The present invention discloses the following technical effects:
[0023] (1) The present invention discloses for the first time a simple preparation method of a high entropy perovskite monolithic catalytic device with a three-dimensional ordered macroporous structure. First, a metal sol dispersion containing PS microspheres is prepared, then coated on a honeycomb (ceramic) substrate, and finally calcined to remove the carbon template to obtain a high entropy perovskite catalytic device with a three-dimensional ordered macroporous structure. The preparation method is simple and easy to prepare in large-scale industrial quantities, and realizes a simplified one-step preparation of a high entropy catalyst with a three-dimensional ordered macroporous structure.
[0024] (2) The three-dimensional ordered macroporous high-entropy perovskite monolithic catalytic device prepared by the present invention has a three-dimensional ordered macroporous structure, which enables the catalyst to have good mass transfer and diffusion performance and catalytic oxidation activity. In addition, the three-dimensional ordered macroporous high-entropy perovskite monolithic catalytic device of the present invention has a high configuration entropy, which gives the catalyst a severe lattice distortion and rich defects, so that the catalyst has excellent catalytic combustion activity and stability (good high temperature resistance, moisture resistance, and sulfur resistance).
[0025] (3) The active components of the catalyst involved in the present invention are low in price, and the catalyst has good economic efficiency. The promotion of the catalyst has huge economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 The physical image, scanning electron microscope image, X-ray diffraction image (XRD) and EDS-Mapping spectrum of HEPO of the catalytic device prepared in Example 1; wherein a is the physical image, b is the scanning electron microscope image, c is the X-ray diffraction image, and d is the EDS-Mapping spectrum;
[0028] Figure 2 This is a graph showing the combustion performance of soot particles catalyzed by the catalytic device prepared in Example 2;
[0029] Figure 3 This is a graph showing the catalytic methane combustion performance of the catalytic device prepared in Example 3;
[0030] Figure 4 This is a graph showing the catalytic combustion performance of propylene by the catalytic device prepared in Example 4;
[0031] Figure 5 This is a physical picture of the macro-quantitative preparation of the catalytic device of Example 3;
[0032] Figure 6 Thermal stability and moisture resistance of the catalytic device prepared in Example 3;
[0033] Figure 7 The catalytic methane combustion performance diagram of the catalytic devices prepared in Example 3 and Comparative Examples 1 and 2;
[0034] Figure 8 The cyclic stability of the catalytic device prepared in Example 3;
[0035] Fig. 9 This is a diagram showing the catalytic methane combustion performance of the catalytic device prepared in Example 3 and other entropy catalytic devices with different configurations. DETAILED DESCRIPTION
[0036] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0037] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0039] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0040] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0041] The size of the honeycomb ceramic substrate used in the embodiments and comparative examples of the present invention is 1.4×1.4×1.5 cm, and other sizes can also achieve the technical effects of the present invention.
[0042] Example 1
[0043] Take 2g of lanthanum nitrate hexahydrate, 0.4g of nickel nitrate nonahydrate, 0.41g of manganese nitrate tetrahydrate, 0.45g of iron nitrate nonahydrate, 0.56g of cobalt nitrate hexahydrate, and 0.16g of copper nitrate hexahydrate and place them in a 200mL beaker, add 100mL of distilled water, and dissolve the solid completely under ultrasonic action. Add 1.250g of citric acid monohydrate solid and 0.307g of ethylene glycol liquid, stir on a magnetic stirrer for 10 minutes to obtain a mixed metal salt sol. Take 3mL of 10g / L PS (polystyrene) microsphere ethylene glycol dispersion and add it to the above mixed metal salt sol, stir for 24 hours to obtain a dispersion. Place the honeycomb ceramic substrate in the above dispersion and immerse and coat for 24 hours, take it out and dry it at 60℃ for 12 hours, and then calcine it at 900℃ for 10 hours to obtain a three-dimensional ordered macroporous high entropy perovskite (3DOMLa(NiMnFeCoCu)O 3) Monolithic catalytic device (abbreviated as: catalytic device, 3DOMHEPO), catalyst loading 4%, pore size 0.5-2μm, porosity 3%.
[0044] The physical image, scanning electron microscope image, X-ray diffraction image (XRD), and EDS-Mapping spectrum of HEPO prepared in this example are as follows: Figure 1 As shown in the figure, a is a physical image, b is a scanning electron microscope image, c is an X-ray diffraction image, and d is an EDS-Mapping spectrum. Figure 1 It can be seen that the catalytic device prepared in this example has a microscopic morphology characteristic of a three-dimensional ordered macroporous structure. No phase separation occurs in the XRD spectrum, further proving the successful preparation of high entropy perovskite oxide (HEPO).
[0045] Example 2
[0046] Take 2.2g of lanthanum nitrate hexahydrate, 0.4g of chromium nitrate nonahydrate, 0.41g of manganese nitrate tetrahydrate, 0.45g of iron nitrate nonahydrate, 0.56g of bismuth nitrate hexahydrate, and 0.13g of copper nitrate hexahydrate and place them in a 500mL beaker, add 200mL of distilled water, and dissolve the solid completely under ultrasonic action. Add 1.240g of citric acid monohydrate solid and 0.307g of ethylene glycol liquid, and stir on a magnetic stirrer for 10 minutes to obtain a mixed metal salt sol. Take 3mL of 10g / L PS microsphere ethylene glycol dispersion and add it to the above mixed metal salt sol, stir for 20 hours to obtain a dispersion. Place the honeycomb ceramic substrate in the above dispersion and immerse and coat for 24 hours, take it out and dry it at 70℃ overnight, and then calcine it at 800℃ for 10 hours to obtain a three-dimensional ordered macroporous high entropy perovskite monolithic catalytic device 3DOMLa(CrMnFeCuBi)O 3 (Abbreviation: catalytic device, 3DOMHEPO), catalyst loading 10%, pore size 0.5-2μm, porosity 3%.
[0047] The catalytic combustion performance of the catalytic device prepared in this example on diesel exhaust soot particles was evaluated and verified, and the evaluation method was as follows:
[0048] The catalytic oxidation activity test of the catalyst sample soot was carried out in a fixed-bed microreactor at normal pressure. The reactor material is a quartz tube with an inner diameter of 6.4mm. The heating program and heating rate are automatically controlled by setting the program. The test heating program is: room temperature → 200℃, residence time is 30min; 200℃ → 700℃, heating rate is 2℃ / min; finally stay at 700℃ for 30min. The soot selected in the experiment is Wuling carbon black particles. The specific soot loading operation is: a certain amount of soot is dissolved in ethylene glycol solution to obtain a 12mg / mL suspension, and a certain amount of suspension is evenly dripped on the sample to be tested with a pipette. Dry at 200℃ to simulate the loose contact mode. The mass ratio of catalyst to soot is maintained at 10 / 1. Subsequently, the sample loaded with soot is wrapped with a quartz wool pad and placed in the constant temperature zone of the reaction tube. The reaction gas composition (volume fraction) is: 10% O 2 , 90% N 2 , the total gas flow rate is 50mL / min.
[0049] The gas content after the reaction was analyzed online using a Fuli GC-9790 gas chromatograph, with FID as the detector, high-purity nitrogen as the carrier gas, column furnace temperature of 90°C, detector temperature of 150°C, and auxiliary temperature of 350°C. The relative peak area of the chromatogram is used to represent the relative content of a certain gas. The catalytic performance is evaluated by T10 and T50, which correspond to the temperatures when the soot conversion rate is 10% and 50%, respectively. The soot conversion rate is calculated as follows: the soot corresponding to a certain temperature and the temperature before that is converted into CO x The peak area is divided by the total soot conversion into CO during the reaction. x The sum of the peak areas.
[0050] Test results such as Figure 2 As shown in the figure, T 90 The temperature required for the soot conversion rate to reach 90% is Figure 2 It can be seen that the catalytic device prepared in Example 2 exhibits good soot catalytic combustion activity, soot is completely oxidized at 550°C, and the catalyst is completely regenerated.
[0051] Example 3
[0052] 0.5g of lanthanum nitrate hexahydrate, 0.11g of calcium nitrate, 0.11g of strontium nitrate, 0.12g of potassium nitrate, 0.02g of bismuth nitrate, 0.4g of chromium nitrate nonahydrate, 0.41g of manganese nitrate tetrahydrate, 0.45g of iron nitrate nonahydrate, 0.56g of cobalt nitrate hexahydrate, and 0.13g of nickel nitrate hexahydrate were placed in a 500mL beaker, and 190mL of distilled water was added. The solid was completely dissolved under ultrasonic action. 1.140g of oxalic acid monohydrate solid and 1.407g of ethylene glycol liquid were added, and the mixed metal salt sol was prepared by stirring on a magnetic stirrer for 60 minutes. 10mL of 10g / L PS microsphere ethylene glycol dispersion was added to the above mixed metal salt sol, and stirred for 1 hour to obtain a dispersion. The honeycomb ceramic substrate was immersed in the above dispersion for 1 hour, dried at 80 °C overnight, and then calcined at 900 °C for 20 hours to finally obtain a three-dimensional ordered macroporous high-entropy perovskite monolithic catalytic device 3DOM(LaCaSrKBi)(CrMnFeCoNi)O containing 10 elements. 3 (Abbreviation: catalytic device, 3DOMHEPO), catalyst loading 10%, pore size 0.5-2μm, porosity 3%.
[0053] The catalytic combustion performance of the catalytic device prepared in this example on coal mine gas methane was evaluated and verified, and the evaluation method was as follows:
[0054] CH 4 The catalytic combustion activity was evaluated using a quartz tube to simulate a fixed bed reactor. The catalyst sample to be tested was loaded in the middle of the quartz tube. The quartz tube was loaded into a tubular furnace, the gas line was connected and leak-checked, and the heating program was set: heating from 25°C to 250°C for 30 minutes, keeping warm for 25 minutes, heating to 300°C at a rate of 10°C / min and keeping warm for 25 minutes, and passing through 350°C-750°C at the same heating rate and keeping warm time. Air was simulated to pass through the catalyst, with a total gas flow rate of 50 mL / min, and 1% CH 4 , 5% O 2 and 94% N 2 The tail gas components of the catalytic reaction were monitored online in real time by gas chromatography (GC-9790). The instrument setting conditions of GC were: carrier gas was N 2 , using a hydrogen flame ionization detector (FID) with a column oven temperature of 70°C. 4 The conversion formula is:
[0055]
[0056] Among them, X in the formula methane represents the conversion rate of methane, F methane,in represents the inlet concentration of methane, F methane,out represents the outlet concentration of methane after catalytic oxidation, Fmethane,in -F methane,out Indicates the concentration of methane converted during catalytic oxidation. 90 It indicates the temperature at which the methane conversion rate reaches 90%.
[0057] Test results such as Figure 3 As shown in the figure, round1 indicates that the catalyst is used in the first round, round2 indicates that the catalyst is used in the second round, and round3 indicates that the catalyst is used in the third round. Figure 3 It can be seen that the catalytic device prepared in Example 3 exhibits good methane catalytic combustion activity, and methane is completely oxidized at 600° C. In addition, the catalyst exhibits good high temperature stability, and the activity does not decrease after 50 hours of use.
[0058] Figure 6 The thermal stability and moisture resistance of the catalytic device prepared in Example 3; Figure 6 It can be seen that the high entropy perovskite prepared in Example 3 can maintain good catalytic activity after thermal aging in air atmosphere at 800°C and 10% humidity. 4 Oxidation to CO 2 The conversion rate has not decreased.
[0059] Figure 8 The cyclic stability of the catalytic device prepared in Example 3; Figure 8 It can be seen that the three-dimensional ordered macroporous high entropy perovskite catalytic device (3DOMHEPO) prepared in Example 3 catalyzes CH 4 Oxidation to CO 2 There was no decrease in catalytic combustion activity.
[0060] Example 4
[0061] Take 1g of lanthanum nitrate hexahydrate, 0.4g of chromium nitrate nonahydrate, 0.41g of manganese nitrate tetrahydrate, 0.45g of iron nitrate nonahydrate, 0.56g of bismuth nitrate hexahydrate, and 0.16g of copper nitrate hexahydrate and place them in a 200mL beaker, add 100mL of distilled water, and dissolve the solid completely under ultrasonic action. Add 1.450g of oxalic acid monohydrate solid and 0.307g of ethylene glycol liquid, and stir on a magnetic stirrer for 10 minutes to obtain a mixed metal salt sol. Take 20ml of 10g / L PS microsphere ethylene glycol dispersion and add it to the above mixed metal salt sol, stir for 24 hours to obtain a dispersion. Place the honeycomb ceramic substrate in the above dispersion and dip-coat it for 10 hours, take it out and dry it at 100℃ overnight, and then calcine it at 760℃ for 10 hours to finally obtain a three-dimensional ordered macroporous high-entropy perovskite monolithic catalytic device 3DOMLa(CrMnFeBiCu)O 3(Abbreviation: catalytic device, 3DOMHEPO), catalyst loading 10%, pore size 0.5-2μm, porosity 4%.
[0062] The catalytic combustion performance of the catalytic device prepared in this example on VOCs (propylene) was evaluated and verified. The evaluation method was: C 3 H 8 The catalytic oxidation activity was evaluated using a quartz tube to simulate a fixed bed reactor. The catalyst sample to be tested was loaded into the middle of the quartz tube, and the temperature was programmed to heat from 200°C to 700°C (5°C / min; 50°C / stage), with each temperature stage maintained for 30 minutes. The composition of the reaction gas was 3000ppmC 3 H 8 , 12% O 2 and N 2 Balance, the total flow rate is 50mL / min, and the corresponding mass space velocity is about 37500mLg -1 h -1 The tail gas components of the catalytic reaction were monitored online in real time by gas chromatography (GC-9790) of Taizhou Fuli Company. 2 The instrument setting conditions of GC-9790 are: carrier gas is N 2 , using a hydrogen flame ionization detector (FID), column furnace temperature 90 ° C, detection temperature 150 ° C, injection temperature 200 ° C, the relative content displayed by the chromatogram is used to represent the concentration of propane. 3 H 8 The conversion formula is:
[0063]
[0064] Among them, X in the formula 丙烯 represents the conversion rate of propylene, F 丙烯,in represents the inlet concentration of propylene, F 丙烯,out represents the outlet concentration of propylene after catalytic oxidation, F 丙烯,in -F 丙烯,out Indicates the concentration of propylene converted during catalytic oxidation.
[0065] Test results such as Figure 4 As shown, from Figure 4 It can be seen that the catalytic device prepared in Example 4 exhibits good propylene catalytic combustion activity, and propylene is completely oxidized at 300° C. In addition, the catalyst exhibits good high temperature stability, and the activity does not decrease after 50 hours of use.
[0066] Comparative Example 1
[0067] La(Mn 0.2 Fe 0.2 Ni0.2 Cu 0.2 Co 0.2 ) 3 The preparation method of the @PAC monolithic catalyst comprises the following steps:
[0068] Dissolve 1mmol of citric acid in 5mL of anhydrous ethanol and stir until it is completely dissolved. Then weigh 1mmol of lanthanum nitrate, 0.2mmol of cobalt nitrate, 0.2mmol of manganese nitrate, 0.2mmol of iron nitrate, 0.2mmol of nickel nitrate, and 0.2mmol of copper nitrate and add them to the above solution respectively. Stir until it is clear and continue stirring for 0.5h to obtain a precursor solution. Use a pipette to transfer 5mL of the precursor solution and drop it on the substrate material. After standing at room temperature for 0.5h, dry it at 80℃ in a forced air drying oven for 2h, and then place it in a muffle furnace and calcine it at 600℃ for 3h to obtain a high entropy perovskite monolithic catalyst La(Mn) with an active component loading of 0.6%. 0.2 Fe 0.2 Ni 0.2 Cu 0.2 Co 0.2 ) 3 @PAC.
[0069] Comparative Example 2
[0070] La(Mn 0.2 Fe 0.2 Ni 0.2 Cu 0.2 Co 0.2 ) 3 The preparation method of the @PAC three-dimensional ordered macroporous monolithic catalyst comprises the following steps:
[0071] Dissolve 1mmol of citric acid in 5mL of anhydrous ethanol and stir until it is completely dissolved. Then weigh 1mmol of lanthanum nitrate, 0.2mmol of cobalt nitrate, 0.2mmol of manganese nitrate, 0.2mmol of iron nitrate, 0.2mmol of nickel nitrate, and 0.2mmol of copper nitrate and add them to the above solution respectively. Stir until it is clear and continue stirring for 0.5h to obtain a precursor solution. Take 20ml of 10g / L PS microsphere ethylene glycol dispersion and add it to the above precursor solution. Stir for 24 hours to obtain a dispersion. Use a pipette to transfer 5mL of the dispersion droplets and apply them on the substrate material. After standing at room temperature for 0.5h, dry it at 80℃ in a forced air drying oven for 2h, and then calcine it at 600℃ in a muffle furnace for 3h to obtain a three-dimensional ordered macroporous high entropy perovskite monolithic catalyst 3DOM La(Mn) with an active component loading of 0.6%. 0.2 Fe 0.2 Ni 0.2 Cu 0.2 Co 0.2) 3 @PAC.
[0072] Figure 5 This is a physical picture of the macro-quantitative preparation of the catalytic device of Example 3;
[0073] Figure 7 The catalytic methane combustion performance diagram of the catalytic device prepared in Example 3 and Comparative Examples 1 and 2 is shown in FIG. Figure 7 It can be seen that the catalytic combustion activity of the catalytic device prepared in Example 3 is relatively high, and the catalytic combustion T90 of catalytic methane is 500°C, while the catalytic combustion T90 of the catalytic device of Comparative Example 1 is 700°C, and the catalytic combustion T90 of the catalytic device of Comparative Example 2 is about 600°C. The three-dimensional ordered macroporous structure of the high entropy catalytic device of the present invention has a significant promoting effect on the catalytic activity. The multiple elements selected in the high entropy catalytic device of the present invention have a large configuration entropy that promotes the activity of the catalyst. The three-dimensional ordered macroporous structure and the high entropy structure work together to significantly reduce the catalytic conversion temperature T90 of the catalyst (700°C→500°C).
[0074] Fig. 9 The catalytic methane combustion performance diagram of the catalytic device prepared in Example 3 and other entropy catalytic devices with different configurations; Fig. 9 It can be seen that the high entropy catalytic device of the present invention exhibits better catalytic combustion activity than traditional low entropy and medium entropy perovskites. As the configuration entropy increases, the T90 conversion temperature of the catalyst decreases significantly (700°C→500°C).
[0075] Catalyst catalytic oxidation of motor vehicle exhaust (CO, NO, CH x During the process of catalyst catalysis, the catalytic activity is affected by the contact efficiency between the reactants and the catalyst and the intrinsic activity of the active sites of the catalyst. The mass transfer and diffusion process of the reactants on the catalyst surface will have a significant impact on the performance of the catalyst. The present invention improves the contact efficiency between the reactants and the catalyst and improves the reaction activity of the catalyst by preparing a three-dimensional ordered macroporous structure on the monolithic catalytic device.
[0076] So far, the research on high entropy materials is still at the laboratory stage, lacking a mild, feasible and easy-to-scale preparation method. The present invention provides a mild, feasible and easy-to-scale preparation method (such as Figure 5 ) and synthesized a monolithic high-entropy perovskite catalytic device with a three-dimensional ordered macroporous microstructure, which is used in the field of environmental thermal catalysis and has a good catalytic oxidation effect.
[0077] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A high entropy perovskite monolithic catalytic device, characterized in that: The high entropy perovskite monolithic catalytic device comprises a substrate and a high entropy perovskite oxide; the high entropy perovskite oxide is loaded on the surface of the substrate; the high entropy perovskite oxide is a three-dimensional ordered macroporous structure; the chemical formula of the high entropy perovskite oxide is ABO3, wherein the A element is selected from one or more of Ca, K, La, Sr, Bi, Gd, Nd, Sm, and Y; the B element is selected from one or more of Cr, Mn, Fe, Co, Ni, Cu, Ti, and Al; at least one of the A element and the B element is composed of five or more elements in an equal molar ratio; The steps for preparing the high entropy perovskite monolithic catalytic device include: A salt containing element A and a salt containing element B are added into water to dissolve, and then an organic acid and an organic solvent are added to obtain a mixed metal salt sol; a polystyrene microsphere dispersion is added to the mixed metal salt sol to obtain a mixed dispersion; a substrate is immersed in the mixed dispersion, and after the immersion is completed, it is dried and calcined to obtain the high entropy perovskite monolithic catalytic device; The loading amount of the high entropy perovskite oxide is 1-20wt%; The substrate is a ceramic substrate or a metal alloy substrate with a honeycomb structure; the pore size of the three-dimensional ordered macroporous structure is 0.5 μm-2 μm, and the porosity is 1%-20%; The salt containing element A is a nitrate of element A; the salt containing element B is a nitrate of element B; the organic acid is oxalic acid, citric acid or fruit acid; the organic solvent is ethylene glycol; the polystyrene microsphere dispersion is a polystyrene microsphere ethylene glycol dispersion; The concentration of the polystyrene microsphere dispersion is 10 g / L; the ratio of the total mass of the salt containing element A and the salt containing element B to the mass of the polystyrene microspheres is 5:1; The impregnation time is 24 hours; the drying is specifically drying at 50° C. for 20 hours; and the calcination is specifically calcining at 800° C. for 48 hours.
2. Use of the high entropy perovskite monolithic catalytic device as claimed in claim 1 in the preparation of a diesel vehicle exhaust particulate matter collector.
3. The use of the high entropy perovskite monolithic catalytic device according to claim 1 in the catalytic combustion purification of VOCs in coal chemical industry, characterized in that: The temperature of catalytic combustion purification is 150-400℃.
4. The use of the high entropy perovskite monolithic catalytic device according to claim 1 in the catalytic combustion purification of methane in coal mine ventilation gas, characterized in that: The temperature of catalytic combustion purification is 350-600℃.
Citation Information
Cited By
Preparation method of three-dimensional porous high-entropy oxide
CN120864569A