Surface-modified flaky zinc oxide and preparation method thereof

By using alkali solution and anionic surfactant to modify zinc salt solution under mild conditions, hydrophobic flake zinc oxide was prepared, which solved the problems of high-temperature hydrothermal consumption and inorganic alkali wastewater in the prior art, and improved the material Dispersibility and stability simplify the process flow.

CN115849432BActive Publication Date: 2024-12-03JIANGSU NAMEI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211708154.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-12-03
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

The existing preparation methods for flake zinc oxide require hydrothermal processes and high-temperature heat treatment, consume a large amount of inorganic alkali, generate a large amount of low-concentration alkaline wastewater, and do not consider organic surface modification, affecting dispersion and stability.

Method used

Prepare alkali solution and add zinc salt solution under mild conditions. Surface modification is carried out by filtration, washing, drying and pulverizing, combined with anionic surfactant, to control the morphology and surface properties of zinc oxide, and achieve hydrophobic flaky zinc oxide. Preparation.

Benefits of technology

While achieving efficient synthesis of sheet zinc oxide and organic surface modification, energy consumption is reduced, process is simplified, dispersion and stability are improved, and application performance of materials is improved through hydrophobic modification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115849432B_ABST
    Figure CN115849432B_ABST
Patent Text Reader

Abstract

The invention discloses an integrated preparation method for the preparation of flaky zinc oxide and its surface modification, wherein an anionic surfactant is added to an alkaline solution to play a dual role of controlling the morphology of zinc oxide and organic surface modification, and the prepared flaky zinc oxide has good hydrophobicity. The invention completes the two processes of the synthesis of flaky zinc oxide and the organic surface modification in one step, with mild conditions, short process and simple operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of inorganic non-metallic novel functional materials and daily chemical industry, and specifically relates to a method for preparing flaky zinc oxide and preparing flaky zinc oxide by organic surface modification. Background Art

[0002] Nano zinc oxide is an important inorganic UV shielding material, which has a good shielding effect on both long-wave ultraviolet rays (UVA) and medium-wave ultraviolet rays (UVB) in sunlight. The microscopic morphology and surface properties of zinc oxide determine its application effect in sunscreen cosmetics and customer acceptance. Compared with granular nano zinc oxide, flake zinc oxide has the characteristics of good skin feel and easy dispersion.

[0003] Chinese patent ZL201810446334.X uses a certain mass ratio of zinc sulfate, urea and hexadecyltrimethylammonium bromide to add to water in turn to form an aqueous solution of a certain concentration, and then washes and centrifuges after a period of constant temperature reaction in the reactor, and obtains two-dimensional leaf-shaped nano zinc oxide after drying at a certain temperature and high-temperature heat treatment. This method requires a hydrothermal process and high-temperature heat treatment. Chinese patent ZL201711404151.3 uses alkali dissolution to form a zinc alkali solution, promotes crystallization through dilution to form a flaky precipitate, and then improves the dispersibility of the flaky ZnO through aging, and finally obtains a flaky ZnO powder product with a diameter of 0.1 to 1.5 μm and a thickness of 0.02 μm to 0.3 μm. Although this method is simple to operate, the alkali dissolution of zinc oxide requires a large amount of inorganic alkali, and the subsequent dilution of the zinc alkali solution with water will produce a large amount of low-concentration alkaline wastewater, and the energy consumption of the concentration and recovery process is high, and the environmental pressure is high.

[0004] Organic surface modification is rarely considered in the existing literature on the preparation of flaky zinc oxide. In fact, in order to improve the dispersibility, compatibility and stability of zinc oxide in sunscreen cosmetics, most zinc oxide in cosmetics must undergo organic surface modification before use. Summary of the invention

[0005] In view of the problems existing in the background technology, the present invention proposes an integrated method for the preparation and surface modification of flaky zinc oxide. The technical solution adopted by the present invention is as follows:

[0006] 1. Preparation of alkaline solution: Add alkali and anionic surfactant to deionized water to prepare an alkaline mixed solution.

[0007] 2. Add a 0.5-2 mol / L zinc salt solution to the alkaline mixed solution in step 1 at 10-30° C. until the pH value is 6-8, heat to 60-75° C., keep stirring for 5-10 hours, filter, wash with deionized water, dry, and crush to obtain a hydrophobic flaky zinc oxide powder.

[0008] Furthermore, the base in step (1) is one or both of sodium hydroxide and potassium hydroxide;

[0009] The anionic surfactant described in step (1) is one or two of sodium stearate, potassium stearate, sodium laurate, potassium laurate, sodium oleate and potassium oleate;

[0010] The concentration of the alkaline mixed solution in step (1) is 1 to 4 mol / L, wherein the molar ratio of the anionic surfactant to the alkali is 0.006 to 0.02:1.

[0011] Furthermore, the zinc salt in step (2) is one or more of zinc chloride, zinc acetate, zinc nitrate and zinc sulfate.

[0012] Beneficial effects of the present invention:

[0013] 1. The anionic surfactant of the present invention plays a dual role as a zinc oxide morphology controller and an organic surface modifier.

[0014] 2. The present invention simultaneously completes the two processes of synthesis of flaky zinc oxide and organic surface modification, with mild conditions, short process and simple operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a SEM photo of the product obtained in Example 1;

[0016] Figure 2 This is a SEM photo of the product obtained in Example 2;

[0017] Figure 3 This is a SEM photo of the product obtained in Example 3;

[0018] Figure 4 The following are the X-ray diffraction patterns of the products obtained in Examples 1 to 3. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below in conjunction with embodiments: These embodiments are only used to illustrate the present invention and are not used to limit the scope of the invention.

[0020] The following examples are water contact measurement methods: LSA60 optical contact angle surface analyzer (LAUDA Scientific, Germany) was used to analyze the hydrophobic properties of the composite surface after surface modification. The tableting method was selected, and 3 g of the sample powder to be tested was pressed into tablets by a tablet press, and then placed on a sample platform for image analysis water contact angle test. The droplet volume remained unchanged (5 μL), and the test position was changed. The experiment was repeated 3 times in parallel and the average value was taken.

[0021] Example 1

[0022] 1. Preparation of alkaline solution: Add 10 mol of sodium hydroxide and 0.06 mol of sodium stearate to deionized water to prepare an alkaline mixed solution with a sodium hydroxide concentration of 1 mol / L.

[0023] 2. At 10°C, add 0.5 mol / L zinc sulfate solution to the alkaline mixed solution in step 1 until the pH value is 6, raise the temperature to 60°C, keep stirring for 10 hours, filter, wash with deionized water, dry, and crush to obtain hydrophobic flaky zinc oxide powder, the water contact angle of the powder tablet is 121.6 degrees.

[0024] Example 2

[0025] 1. Preparation of alkaline solution: Add 10 mol of sodium hydroxide and 0.2 mol of sodium stearate to deionized water to prepare an alkaline mixed solution with a sodium hydroxide concentration of 4 mol / L.

[0026] 2. At 30°C, add 2 mol / L zinc sulfate solution to the alkaline mixed solution in step 1 until the pH value is 8, raise the temperature to 75°C, keep stirring for 10 hours, filter, wash with deionized water, dry, and crush to obtain hydrophobic flaky zinc oxide powder, the water contact angle of the powder tablet is 136.5 degrees.

[0027] Example 3

[0028] 1. Preparation of alkaline solution: Add 10 mol of sodium hydroxide and 0.1 mol of sodium stearate to deionized water to prepare an alkaline mixed solution with a sodium hydroxide concentration of 2 mol / L.

[0029] 2. At 25°C, add 1 mol / L zinc sulfate solution to the alkaline mixed solution in step 1 until the pH value is 6.5, raise the temperature to 70°C, keep stirring for 8 hours, filter, wash with deionized water, dry, and crush to obtain hydrophobic flaky zinc oxide powder, the water contact angle of the powder tablet is 135.3 degrees.

[0030] Example 4

[0031] 1. Preparation of alkaline solution: Add 10 mol of potassium hydroxide and 0.1 mol of sodium laurate to deionized water to prepare an alkaline mixed solution with a potassium hydroxide concentration of 2 mol / L.

[0032] 2. At 22°C, add 1.5 mol / L zinc chloride solution to the alkaline mixed solution in step 1 until the pH value is 7.8, raise the temperature to 66°C, keep stirring for 9 hours, filter, wash with deionized water, dry, and crush to obtain hydrophobic flaky zinc oxide powder, the water contact angle of the powder tablet is 139.7 degrees.

[0033] Comparative Example 1

[0034] 1. Preparation of alkaline solution: Add 10 moles of sodium hydroxide to deionized water to prepare an alkaline solution with a sodium hydroxide concentration of 2 mol / L.

[0035] At 25°C, add 1 mol / L zinc sulfate solution to the alkaline solution in step 1 until the pH value is 6.5, raise the temperature to 70°C, keep stirring for 8 hours, filter, wash with deionized water, dry, and crush to obtain hydrophilic granular zinc oxide powder.

Claims

1. A method for preparing a surface-modified flaky zinc oxide, characterized in that: The steps include: (1) Preparation of alkaline solution: adding alkali and anionic surfactant to deionized water to prepare an alkaline mixed solution; the anionic surfactant is one or two of sodium stearate, potassium stearate, sodium laurate, and potassium laurate; the concentration of the alkali in the alkaline mixed solution is 1 to 4 mol / L, and the molar ratio of the anionic surfactant to the alkali is 0.006 to 0.02:1; (2) adding a zinc salt solution having a concentration of 0.5 to 2 mol / L to the alkaline mixed solution of step (1) at 10 to 30° C. until the pH value reaches 6 to 8, heating to 60 to 75° C., stirring at this temperature for 5 to 10 hours, filtering, washing with deionized water, drying, and pulverizing to obtain a hydrophobic flaky zinc oxide powder.

2. The method for preparing the surface-modified flaky zinc oxide according to claim 1, characterized in that: The alkali in step (1) is one or both of sodium hydroxide and potassium hydroxide.

3. The method for preparing the surface-modified flaky zinc oxide according to claim 1, characterized in that: The zinc salt in step (2) is one or more of zinc chloride, zinc acetate, zinc nitrate and zinc sulfate.

4. A surface-modified flaky zinc oxide, characterized in that: Prepared by the preparation method according to any one of claims 1 to 3.