Electrode slurry and preparation method thereof, photovoltaic cell

By wrapping the glass material of titanium powder in the electrode slurry, using its metal activity to react with the oxide, slowing down the etching speed, the problem of over-etching of the silicon matrix by the conductive slurry is solved, and the open circuit voltage and photoelectricity of the battery are improved. conversion efficiency.

CN115862926BActive Publication Date: 2024-10-29ZHEJIANG GUANGDA ELECTRONICS TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211459157.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-10-29
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

The oxides of the glass powder in the current conductive paste on the front of the Topcon battery cause excessive etching of the silicon nitride anti-reflective film layer, affecting the open voltage and photoelectric conversion efficiency of the battery.

Method used

The electrode slurry uses silver-based conductive material, glass material, organic carrier and titanium powder. The glass material wraps the titanium powder. The metal activity of the titanium powder reacts with the oxide to slow down the possibility of the glass material penetrating the anti-reflection layer and avoid Over-etching and improved oxidation resistance.

Benefits of technology

It effectively avoids excessive etching of the silicon substrate by the electrode slurry, reduces leakage and emitter defects, and improves the open circuit voltage and photoelectric conversion efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115862926B_ABST
    Figure CN115862926B_ABST
Patent Text Reader

Abstract

The present invention discloses an electrode slurry, a preparation method and a photovoltaic cell, and relates to the technical field of solar cells, in order to solve the problem that the existing electrode slurry is easy to cause etching to the silicon substrate during the battery manufacturing process, thereby affecting the battery conversion efficiency. The electrode slurry includes: a silver-based conductive material, a glass material, an organic carrier and titanium powder, the glass material contains an oxide, and the glass material wraps the titanium powder. The preparation method is used to prepare the electrode slurry, and the photovoltaic cell uses the electrode slurry. The electrode slurry, the preparation method and the photovoltaic cell provided by the present invention are used to improve the photoelectric conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to an electrode slurry and a preparation method thereof, and a photovoltaic cell. Background Art

[0002] Solar photovoltaic utilization is one of the fastest growing projects in recent years. Silicon is the most ideal solar cell material. For this reason, people have studied and developed crystalline silicon solar cells. Although the current production capacity, technology, and industrial chain are more mature and complete, the difficulty of realization still exists. Improving the conversion efficiency of crystalline silicon solar cells is particularly important. N-type cells are increasingly favored by people and the market due to their advantages such as low light attenuation coefficient, insensitivity to metal impurities, low temperature coefficient, weak light response, etc., especially the introduction of new battery processes and technologies such as tunnel oxide passivated contact (Tunnel Oxide Passivated Contact, Topcon).

[0003] The conductive paste used on the front of the existing Topcon battery often contains glass powder. Glass powder is one of the main components of silver paste. It can affect the electrical properties and photoelectric conversion efficiency of solar cells by adjusting the performance of silver paste. After the glass powder is melted, it can bond the silver powder and can also serve as a sintering aid to reduce the sintering temperature. The oxide of the glass powder system in the positive silver paste system has a certain corrosive ability and can melt and etch the anti-reflection layer on the top of the silicon substrate, so that the silver powder forms an ohmic contact with the silicon substrate. However, due to the presence of oxides in the glass powder, it is easy to over-etch when using conductive paste to etch the silicon nitride anti-reflection film layer, resulting in the etching of the silicon substrate of the Topcon battery, affecting the opening voltage of the battery and reducing the conversion efficiency of the battery. Therefore, it is very important to solve the above problems. Summary of the invention

[0004] The purpose of the present invention is to provide an electrode slurry and a preparation method thereof, and a photovoltaic cell, which can avoid etching the silicon substrate when etching the silicon nitride anti-reflection film layer during the cell manufacturing process, thereby improving the photoelectric conversion efficiency.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] An electrode slurry comprises: a silver-based conductive material, a glass material, an organic carrier and titanium powder, wherein the glass material contains oxides and the glass material wraps the titanium powder.

[0007] Compared with the prior art, in the first aspect, the electrode slurry provided by the present invention has the following advantages:

[0008] The electrode slurry provided by the present invention includes a silver-based conductive material, a glass material, an organic carrier and titanium powder. Among them, because the glass material contains oxides, it has a certain corrosive ability and can melt and etch the anti-reflection layer on the upper part of the silicon substrate, so that the silver powder forms an ohmic contact with the silicon substrate. When the glass material wraps the titanium powder, due to the strong metallic activity of the titanium powder, the oxide in the glass material can react with the titanium powder. Therefore, when the electrode slurry is sintered to etch the anti-reflection layer, the possibility of the glass material penetrating the anti-reflection layer can be slowed down, thereby avoiding excessive etching of the silicon substrate by the electrode slurry, and can also reduce the probability of defects in the emitter, thereby reducing leakage, thereby increasing the open circuit voltage of the battery. The titanium powder contained in the electrode slurry of the embodiment of the present invention also has a strong antioxidant property. Therefore, when the glass material wraps the titanium powder, the antioxidant property of the electrode slurry of the embodiment of the present invention can be improved.

[0009] It can be seen from the above that the electrode slurry provided by the present invention can reduce the possibility of the anti-reflection layer being penetrated during the process of forming electrode grid lines on the battery cell, thereby avoiding excessive etching of the silicon substrate by the electrode slurry and emitter surface defects caused by metal surface recombination, thereby reducing leakage and improving photoelectric conversion efficiency.

[0010] In a second aspect, the present invention further provides a method for preparing an electrode slurry, comprising:

[0011] The titanium powder is wrapped with a glass material to obtain a premix;

[0012] The resin, the solvent and the surface dispersant are mixed, and fumed silica is added to the mixture to obtain an organic carrier;

[0013] The organic carrier is mixed with a silver-based conductive material, a premix, an aluminum-based conductive material and a metal additive to obtain an electrode slurry.

[0014] Compared with the prior art, the beneficial effects of the method for preparing the electrode slurry in the photovoltaic cell provided by the present invention are the same as the beneficial effects of the electrode slurry in the first aspect, which will not be described in detail here.

[0015] In a third aspect, the present invention further provides a photovoltaic cell, wherein the surface of the photovoltaic cell has grid lines, and the material of the grid lines is the electrode slurry provided by the present invention.

[0016] Compared with the prior art, the material of the grid lines in the photovoltaic cell provided by the present invention is the electrode slurry provided by the present invention, so the beneficial effects are the same as those of the electrode slurry in the first aspect, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0018] Figure 1 The figure is a flow chart of the preparation of the electrode slurry according to an embodiment of the present invention. DETAILED DESCRIPTION

[0019] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0020] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.

[0021] The photovoltaic cell industry belongs to the midstream of the photovoltaic industry chain. It is made from silicon wafers through steps such as cleaning and texturing. Photovoltaic panels generate voltage and current under light, thereby realizing photovoltaic power generation. Depending on the raw materials and battery preparation technology, photovoltaic cells can be divided into P-type cells and N-type cells. P-type silicon wafers are made by doping boron in silicon materials. N-type silicon wafers are made by doping phosphorus in silicon materials. P-type cell preparation technologies include traditional aluminum back field and PERC technology. There are many N-type cell preparation technologies, including Practical Extraction and Report Language (PERT / PERL), TOPCon, IBC and heterojunction (Heterojunction with Intrinsic Thinfilm, HJT).

[0022] N-type batteries have high conversion efficiency and are expected to replace P-type batteries and become the mainstream technology of photovoltaic cells in the future. Theoretically, N-type batteries have obvious advantages. Compared with traditional P-type monocrystalline batteries and P-type polycrystalline batteries, N-type batteries have the advantages of high conversion efficiency, high bifaciality, low temperature coefficient, no light decay, good weak light effect, and longer carrier life. Its battery process and efficiency improvement have been significantly accelerated, and there is more room for improvement in conversion efficiency in the future. According to the Photovoltaic Association's industrial development route report, the conversion efficiency of N-type high-efficiency batteries may exceed 25.5% in 2030, which is more than 1 percentage point higher than that of P-type batteries. As the cost of domestic equipment continues to decrease and the efficiency improvement space of N-type batteries has advantages, the pursuit of more efficient batteries has also become the choice of the market and is expected to become the development direction of the next generation of battery technology.

[0023] Photovoltaic cell metallization is an extremely critical part of photovoltaic cell manufacturing. A good metallization paste can greatly improve the efficiency and performance of the entire cell. For existing N-type cells, glass powder is often added to the conductive paste used on the front of the cell. Glass powder is one of the main components of silver paste, which can affect the electrical properties and photoelectric conversion efficiency of solar cells by adjusting the properties of silver paste. However, due to the presence of oxides in the glass powder, it is easy to over-etch when using conductive paste to etch the silicon nitride anti-reflection film layer, resulting in etching of the silicon substrate of the N-type cell, affecting the opening voltage of the cell and reducing the conversion efficiency of the cell.

[0024] In view of the above problems, an embodiment of the present invention provides a photovoltaic cell, the surface of which has a grid line, and the material of the grid line is the electrode slurry provided in the embodiment of the present invention, so as to provide a photovoltaic cell that avoids etching the silicon substrate when etching the silicon nitride anti-reflection film layer during the cell manufacturing process, thereby improving the photoelectric conversion efficiency. It should be understood that the photovoltaic cell can be a Topcon cell, an Interdigitated back contact (IBC) cell or a heterojunction cell, or other photovoltaic cells, which will not be described in detail here.

[0025] An electrode slurry provided in an embodiment of the present invention includes: a silver-based conductive material, a glass material, an organic carrier and titanium powder, wherein the glass material contains an oxide and the titanium powder is wrapped by the glass material. It should be understood that the wrapping here means that a single titanium powder or a plurality of titanium powders are wrapped by the glass powder, and the aluminum-based conductive material can be at least one of aluminum powder, aluminum-silicon alloy powder or other aluminum alloy materials, which is not limited here.

[0026] The electrode slurry provided by the present invention includes a silver-based conductive material, a glass material, an organic carrier and titanium powder. Among them, because the glass material contains oxides, it has a certain corrosive ability and can melt and etch the anti-reflection layer on the upper part of the silicon substrate, so that the silver powder forms an ohmic contact with the silicon substrate. When the glass material wraps the titanium powder, due to the strong metallic activity of the titanium powder, the oxide in the glass material can react with the titanium powder. Therefore, when the electrode slurry is sintered to etch the anti-reflection layer, the possibility of the glass material penetrating the anti-reflection layer can be slowed down, thereby avoiding excessive etching of the silicon substrate by the electrode slurry, and can also reduce the probability of defects in the emitter, thereby reducing leakage, thereby increasing the open circuit voltage of the battery. The titanium powder contained in the electrode slurry of the embodiment of the present invention also has a strong antioxidant property. Therefore, when the glass material wraps the titanium powder, the antioxidant property of the electrode slurry of the embodiment of the present invention can be improved.

[0027] It can be seen from the above that the electrode slurry provided by the present invention can reduce the possibility of the anti-reflection layer being penetrated during the process of forming electrode grid lines on the battery cell, thereby avoiding excessive etching of the silicon substrate by the electrode slurry and emitter surface defects caused by metal surface recombination, thereby reducing leakage and improving photoelectric conversion efficiency.

[0028] In one achievable manner, the organic carrier of the embodiment of the present invention includes a resin, an organic solvent, a surface dispersant, and a gas-phase inorganic nanomaterial. The organic carrier is a liquid, and the gas-phase inorganic nanomaterial is uniformly dispersed in the organic carrier.

[0029] For the organic carrier, the resin includes one or more of ethyl cellulose, cellulose acetate butyrate, rosin resin, acrylic resin, and polyvinyl butyral. The organic solvent may include pinene alcohol, butyl carbitol, butyl carbitol acetate, diethylene glycol butyl ether acetate, diethylene glycol dibutyl ether, tripropylene glycol monomethyl ether, diisooctyl adipate, diethylene glycol butyl ether, oleic acid, 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, triethylene glycol butyl ether, alcohol fat twelve, and alcohol fat sixteen. The thixotropic agent includes one or more of Thixatrol Max, Thixatrol Plus, Thixatrol ST, and Disparlon 6500. The surfactant and dispersant include one or more of TDO, ED120, BYK111, KYC913, and Solsperse 8600.

[0030] In an optional manner, the organic carrier may contain, by mass percentage, 1% to 6% of ethyl cellulose, 1% to 40% of polyvinyl butyral, 10% to 70% of diethylene glycol butyl ether acetate, 10% to 60% of tripropylene glycol monomethyl ether, 5% to 50% of diethylene glycol dibutyl ether, 0% to 15% of triethylene glycol diisooctanoate, 3% to 15% of diisooctyl adipate, 0% to 30% of diethylene glycol butyl ether, 0% to 30% of pineneol, 0% to 10% of oleic acid, 0% to 20% of 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 0% to 20% of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, 1% to 10% of Thixatrol Max, 0% to 10% hydrogenated castor oil, 0% to 10% TDO, 0% to 10% ED120, 0% to 10% BYK111 and 0% to 10% KYC913.

[0031] As can be seen from the above, the organic carrier of the embodiment of the present invention, since the organic carrier is liquid, can evenly disperse the gas-phase inorganic nano material in the organic carrier, so that the organic carrier can evenly wrap the gas-phase inorganic nano material. It should be understood that the gas-phase inorganic nano material can include at least one of gas-phase silicon dioxide, gas-phase aluminum oxide and gas-phase titanium dioxide, and the gas-phase inorganic nano material accounts for 1% to 30% of the mass ratio of the organic carrier. Therefore, the gas-phase inorganic nano material of the embodiment of the present invention, because it can form a large specific surface area of ​​hydrogen bond or some other structure with the polymer, has a strong thixotropy, can effectively improve the aspect ratio of the linear type, when the gas-phase inorganic nano material is added to the resin, the resin glue can have a higher consistency when it is static, and it becomes a material of low-viscosity fluid under the action of external force, so that the organic carrier reaches the required viscosity.

[0032] On this basis, when an organic carrier containing gas-phase inorganic nanomaterials is added to the embodiment of the present invention, the organic carrier can be integrated with the glass material. Since the gas-phase inorganic nanomaterials have a three-dimensional network structure, they can effectively prevent the movement of the liquid, slow down the flow rate of the glass material, and thus slow down the doping rate of the glass material, resulting in a weakening of the ability of heavy metal doping. Since the slower the doping rate, the lower the doping concentration, the possibility of the glass material penetrating the anti-reflection layer (such as SiNx) can be slowed down, avoiding excessive etching of the silicon substrate by the electrode slurry, and reducing the probability of defects in the emitter, thereby reducing leakage, thereby increasing the open circuit voltage of the battery.

[0033] In an optional manner, the electrode slurry of the embodiment of the present invention further includes an aluminum-based conductive material and a slurry additive, and the slurry additive includes at least one of silicon, magnesium, titanium, zinc, gallium powder, aluminum, tellurium, graphite powder and graphene powder. For example, the slurry additive may include at least one of silicon powder, silicon oxide powder, magnesium powder, magnesium oxide powder, titanium oxide powder, zinc oxide powder, gallium nitride powder, silicon nitride powder, boron nitride powder, aluminum oxide powder, tellurium powder, graphite powder or graphene powder. The slurry additive of the embodiment of the present invention, because of its different boiling point from the silver-based conductive material and the glass powder, can slow down the etching speed of the electrode slurry in the process of forming the electrode grid line on the battery cell, thereby avoiding excessive etching of the silicon substrate by the electrode slurry.

[0034] Exemplarily, the mass ratio of the glass material, organic carrier, titanium powder, silver-based conductive material, aluminum-based conductive material and slurry additive in the embodiment of the present invention is (1-7): (2-28): (0.05-1): (80-92): (0.5-4): (0.05-3). Within this mass ratio range, the embodiment of the present invention can make the oxide in the glass material react with the titanium powder by using a small amount of titanium powder, thereby avoiding the problem of excessive etching of the silicon substrate of the photovoltaic cell by the oxide in the glass material when etching the anti-reflection layer by sintering the electrode slurry.

[0035] As for the glass material, it can be at least one of PbO-B2O3-SiO2-Al2O3 system glass, PbO-B2O3-SiO2-Al2O3-ZnO system glass, V2O5-PbO system glass, Bi2O3-B2O3-SiO2 system glass, PbO-SiO2-Ti2O-ZnO system glass, and PbO-B2O3-SiO2-Fe2O3 system glass, or it can be other system glass, which is not limited here.

[0036] In an optional manner, in the electrode slurry implemented by the present invention, the average particle size of the silver-based conductive material is 0.5μm to 5μm, and the particle size range of the aluminum-based conductive material is 0.5μm to 5μm. The aluminum-based conductive material includes at least one of aluminum and aluminum alloy, and the aluminum alloy includes at least one of aluminum-silicon alloy, aluminum-lead alloy, boron-aluminum alloy, gallium-aluminum alloy and indium-aluminum alloy. In the electrode slurry provided by the embodiment of the present invention, by controlling the average particle size of the silver-based conductive material to 0.5μm to 5μm, and the particle size range of the aluminum-based conductive material to 0.5μm to 5μm, when the main grid is formed on the battery, the problem of the silver-plated glass material with a larger particle size easily blocking the network when the main grid line is narrow and unable to print normally is avoided.

[0037] For the aluminum-based conductive material, it can specifically be aluminum powder or aluminum alloy powder, which is at least one of metallic aluminum powder, boron aluminum alloy powder, aluminum silicon alloy powder, aluminum zinc alloy powder, gallium aluminum alloy powder, indium aluminum alloy powder, 2024 aluminum alloy powder, 7075 aluminum alloy powder, 7050 aluminum alloy powder, 2219 aluminum alloy powder, and 6061 aluminum alloy powder.

[0038] For the silver-based conductive material, it can be any one or two of silver powder, Ag-M alloy powder, and Ag-Cu-N alloy powder, wherein M includes one or more of Al, Au, Ba, Bi, Ca, Cd, Ce, Co, Cr, Cu, Dy, Er, Eu, Fe, Ga, Gd, Ge, Ho, In, Ir, La, Lu, Mg, Mn, Mo, Nd, Ni, Pb, Pd, Pm, Pr, Pt, Re, Rh, Ru, Sb, Sc, Si, Sm, Sn, Sr, Tb, Te, Ti, Tm, Y, Yb, Zn, and Zr; and N includes one or more of P, Zn, Ni, Pb, and Sn.

[0039] Figure 1 The preparation flow chart of the electrode slurry provided by the embodiment of the present invention is shown as follows: Figure 1 As shown, the present invention also provides a method for preparing the above-mentioned electrode slurry, comprising:

[0040] Step 101: Use glass material to wrap titanium powder to obtain a premix.

[0041] For example, the raw materials of the glass material can be placed in a three-dimensional mixer and mixed evenly, and the evenly mixed glass material is placed in an alumina crucible for melting, the melted glass material is quenched, and then titanium powder is added to make the glass material evenly wrap the titanium powder to obtain a premix. When the glass material wraps the titanium powder, the oxide in the glass material can react with the titanium powder due to the strong metallic activity of the titanium powder. Therefore, when the electrode slurry is sintered to etch the anti-reflection layer, the possibility of the glass material penetrating the anti-reflection layer can be reduced, thereby avoiding excessive etching of the silicon substrate by the electrode slurry, and reducing the probability of defects in the emitter, thereby reducing leakage, thereby increasing the open circuit voltage of the battery.

[0042] Step 102: Mix the resin, the organic solvent and the surface dispersant, and add the gas-phase inorganic nanomaterial to mix, so as to obtain an organic carrier.

[0043] For example: the organic solvent and the surface dispersant are mixed and stirred evenly, heated to 80°C for full activation, and then the gas-phase inorganic nanomaterial is added, and then the resin is added and continued to be stirred. After the gas-phase inorganic nanomaterial is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0044] Step 103: Mix the organic vehicle, the premix, the silver-based conductive material, the aluminum-based conductive material and a slurry additive to obtain an electrode slurry.

[0045] For example, the premix, organic carrier, silver-based conductive material, aluminum-based conductive material and slurry additive are mixed and stirred, and the mixed mixture is rolled on a three-roll mill to further disperse and homogenize. When the scraper fineness of the three-roll mill reaches the required fineness, it is filtered to obtain the electrode slurry.

[0046] In an optional manner, a rolling mill can be used to roll the glass material, and a pulverizer can be used to pulverize the rolled glass sheet, and then a vibrating screener can be used to screen the pulverized glass powder, and then an airflow mill can be used to polish, grind and grade the screened glass powder. The rolling mill can be a double-roll rolling mill or a single-roll rolling mill, the pulverizer can be any one of a mechanical pulverizer, an airflow pulverizer, a grinder and a low-temperature pulverizer, the vibrating screener can be a fixed screener or a movable screener, and the airflow mill can be one of a flat airflow mill, a circulating airflow mill, a jet airflow mill, a target airflow mill and a fluidized jet airflow mill.

[0047] The electrode slurry provided by the present invention has a certain corrosive ability because the glass material contains oxides, and can melt and etch the anti-reflection layer on the top of the silicon substrate, so that the silver powder forms an ohmic contact with the silicon substrate. When the glass material wraps the titanium powder, the oxide in the glass material can react with the titanium powder due to the strong metallic activity of the titanium powder. Therefore, when the electrode slurry is sintered to etch the anti-reflection layer, the possibility of the glass material penetrating the anti-reflection layer can be slowed down, thereby avoiding excessive etching of the silicon substrate by the electrode slurry, and can also reduce the probability of defects in the emitter, thereby reducing leakage, thereby increasing the open circuit voltage of the battery. The titanium powder contained in the electrode slurry of the embodiment of the present invention also has a strong antioxidant property. Therefore, when the glass material wraps the titanium powder, the antioxidant property of the electrode slurry of the embodiment of the present invention can be improved.

[0048] In order to verify the effect of the electrode slurry provided by the embodiment of the present invention, the embodiment of the present invention is demonstrated by comparing the embodiment with the comparative example.

[0049] Embodiment 1

[0050] The electrode slurry provided by the embodiment of the present invention includes, by mass percentage, 80% of silver-based conductive material, 0.5% of aluminum-based conductive material, 0.05% of titanium powder, 1% of glass material, 2% of organic carrier and 0.05% of slurry additive.

[0051] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0052] The first step is to prepare glass material: 75% Pb3O4, 17% H3BO3, 7% ZnO, and 1% SiO2 are mixed by mass percentage, melted and quenched at high temperature, and then ground to obtain glass powder with a particle size of D50 = 0.5um ~ 3um, that is, glass material.

[0053] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0054] The third step is to prepare an organic carrier: by mass percentage, 40% of diethylene glycol butyl ether acetate, 10% of diethylene glycol dibutyl ether, 20% of pineol, and 6% of Thixatrol Max are mixed and stirred evenly, heated to 80°C for full activation, and then 15% of fumed silica, 5% of ED120, and 4% of polyvinyl butyral resin are added, and stirring is continued. After the fumed silica is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0055] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0056] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0057] Embodiment 2

[0058] The electrode slurry provided by the embodiment of the present invention includes, by mass percentage, 85% of silver-based conductive material, 2% of aluminum-based conductive material, 0.07% of titanium powder, 3% of glass material, 10% of organic carrier and 1.2% of slurry additive.

[0059] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0060] The first step is to prepare glass material: 75% Pb3O4, 16% H3BO3, 7% ZnO, 1% SiO2, and 1% Al2O3 are mixed by mass percentage, melted and quenched at high temperature, and then ground to obtain glass powder with a particle size of D50 = 0.5um to 3um.

[0061] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0062] The third step is to prepare an organic carrier: by mass percentage, 40% of diethylene glycol butyl ether acetate, 10% of diethylene glycol dibutyl ether, 18% of pineol, and 6% of Thixatrol Max are mixed and stirred evenly, heated to 80°C for full activation, and then 16% of fumed silica, 5% of TDO, 2% of polyvinyl butyral resin, and 2% of ECN4 resin are added and continued to stir. After the fumed silica is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0063] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0064] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0065] Embodiment 3

[0066] The electrode slurry provided by the embodiment of the present invention includes, by mass percentage, 90% of silver-based conductive material, 3% of aluminum-based conductive material, 0.08% of titanium powder, 6% of glass material, 20% of organic carrier and 2% of slurry additive.

[0067] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0068] The first step is to prepare glass materials: 75% Pb3O4, 15% H3BO3, 6% ZnO, 2% SiO2, and 2% V2O5 are mixed by mass percentage, and after high-temperature melting and quenching, the glass powder with a particle size of D50 = 0.5um to 3um is ground.

[0069] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0070] The third step is to prepare an organic carrier: by mass percentage, 40% of diethylene glycol butyl ether acetate, 10% of diethylene glycol dibutyl ether, 20% of pine alcohol, and 6% of Thixatrol Max are mixed and stirred evenly, heated to 80°C for full activation, and then 15% of fumed silica, 5% of ED120, 2% of polyvinyl butyral resin, and 2% of ECN4 resin are added, and stirring is continued. After the fumed silica is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0071] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0072] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0073] Embodiment 4

[0074] The electrode slurry provided by the embodiment of the present invention comprises, by mass percentage, 92% of silver-based conductive material, 4% of aluminum-based conductive material, 1% of titanium powder, 7% of glass material, 28% of organic carrier and 3% of slurry additive.

[0075] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0076] The first step is to prepare glass material: 75% Pb3O4, 17% H3BO3, 7% ZnO, and 1% SiO2 are mixed by mass percentage, melted and quenched at high temperature, and then ground to obtain glass powder with a particle size of D50 = 0.5um to 3um.

[0077] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0078] The third step is to prepare an organic carrier: by mass percentage, 40% of diethylene glycol butyl ether acetate, 10% of tripropylene glycol monomethyl ether, and 6% of Thixatrol Max are mixed and stirred evenly, heated to 80°C for full activation, and then 15% of fumed silica, 4% of ED120, and 5% of polyvinyl butyral resin are added, and stirring is continued. After the fumed silica is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0079] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0080] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0081] Embodiment 5

[0082] The electrode slurry provided by the embodiment of the present invention includes, by mass percentage, 80% of silver-based conductive material, 0.5% of aluminum-based conductive material, 0.05% of titanium powder, 1% of glass material, 2% of organic carrier and 0.05% of slurry additive.

[0083] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0084] The first step is to prepare glass material: 75% PbO and 25% V2O5 are mixed by mass percentage, melted and quenched at high temperature, and then ground to obtain glass powder with a particle size of D50 = 0.5um ~ 3um, that is, glass material.

[0085] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0086] The third step is to prepare an organic carrier: by mass percentage, 6% of ethyl cellulose, 30% of diethylene glycol butyl ether acetate, 10% of diethylene glycol dibutyl ether, 5% of triethylene glycol diisooctanoate, 20% of pinene alcohol, and 6% of ThixatrolMax are mixed and stirred evenly, heated to 80°C for full activation, and then 15% of fumed silica, 5% of ED120, and 4% of polyvinyl butyral resin are added, and stirring is continued. After the fumed silica is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0087] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0088] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0089] Embodiment 6

[0090] The electrode slurry provided by the embodiment of the present invention includes, by mass percentage, 83% of silver-based conductive material, 0.8% of aluminum-based conductive material, 0.06% of titanium powder, 2% of glass material, 5% of organic carrier and 0.1% of slurry additive.

[0091] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0092] The first step is to prepare glass material: 75% PbO, 20% B2O3, 2% SiO2 and 3% Al2O3 are mixed by mass percentage, melted and quenched at high temperature, and then ground to obtain glass powder with a particle size of D50 = 0.5um ~ 3um, that is, glass material.

[0093] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0094] The third step is to prepare an organic carrier: by mass percentage, 3% of ethyl cellulose, 35% of diethylene glycol butyl ether acetate, 10% of diisooctyl adipate, 5% of triethylene glycol diisooctanoate, 20% of pineneol, and 6% of ThixatrolMax are mixed and stirred evenly, heated to 80°C for full activation, and then 10% of fumed silica, 5% of fumed titanium dioxide, 5% of ED120, and 4% of polyvinyl butyral resin are added, and stirring is continued. After the fumed silica is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0095] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0096] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0097] Embodiment 7

[0098] The electrode slurry provided by the embodiment of the present invention includes, by mass percentage, 85% of silver-based conductive material, 0.8% of aluminum-based conductive material, 0.06% of titanium powder, 2% of glass material, 5% of organic carrier and 0.1% of slurry additive.

[0099] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0100] The first step is to prepare glass material: 75% PbO, 20% B2O3, 2% SiO2 and 3% Al2O3 are mixed by mass percentage, melted and quenched at high temperature, and then ground to obtain glass powder with a particle size of D50 = 0.5um ~ 3um, that is, glass material.

[0101] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0102] The third step is to prepare an organic carrier: by mass percentage, 3% of ethyl cellulose, 35% of diethylene glycol butyl ether acetate, 10% of diisooctyl adipate, 5% of triethylene glycol diisooctanoate, 20% of pinene alcohol, and 6% of ThixatrolMax are mixed and stirred evenly, heated to 80°C for full activation, and then 15% of fumed titanium dioxide, 5% of ED120, and 2% of polyvinyl butyral resin are added, and stirring is continued. After the fumed silica is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0103] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0104] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0105] Embodiment 8

[0106] The electrode slurry provided by the embodiment of the present invention includes, by mass percentage, 87% of silver-based conductive material, 0.9% of aluminum-based conductive material, 0.07% of titanium powder, 3% of glass material, 5% of organic carrier and 0.1% of slurry additive.

[0107] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0108] The first step is to prepare glass material: 75% PbO, 20% B2O3, 2% SiO2 and 3% Fe2O3 are mixed by mass percentage, melted and quenched at high temperature, and then ground to obtain glass powder with a particle size of D50 = 0.5um ~ 3um, that is, glass material.

[0109] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0110] The third step is to prepare an organic carrier: by mass percentage, 40% of diethylene glycol butyl ether acetate, 10% of diisooctyl adipate, 5% of triethylene glycol diisooctanoate, 20% of pineneol, and 6% of Thixatrol Max are mixed and stirred evenly, heated to 80°C for full activation, and then 5% of fumed titanium dioxide, 5% of fumed silica, 5% of fumed alumina, 5% of ED120, and 2% of polyvinyl butyral resin are added, and stirring is continued until the fumed silica is evenly stirred and the resin is fully dissolved, and then the organic carrier is obtained after standing and cooling.

[0111] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0112] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0113] Embodiment 9

[0114] The electrode slurry provided by the embodiment of the present invention includes, by mass percentage, 89% of silver-based conductive material, 2% of aluminum-based conductive material, 0.07% of titanium powder, 3% of glass material, 5% of organic carrier and 0.1% of slurry additive.

[0115] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0116] The first step is to prepare glass material: 75% PbO, 20% B2O3, 2% SiO2 and 3% Fe2O3 are mixed by mass percentage, melted and quenched at high temperature, and then ground to obtain glass powder with a particle size of D50 = 0.5um ~ 3um, that is, glass material.

[0117] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0118] The third step is to prepare an organic carrier: by mass percentage, 40% of diethylene glycol butyl ether acetate, 10% of diisooctyl adipate, 5% of triethylene glycol diisooctanoate, 20% of pineneol, and 6% of Thixatrol Max are mixed and stirred evenly, heated to 80°C for full activation, and then 10% of fumed silica, 5% of fumed alumina, 5% of ED120, and 2% of polyvinyl butyral resin are added, and stirring is continued. After the fumed silica is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0119] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0120] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0121] Embodiment 10

[0122] The electrode slurry provided by the embodiment of the present invention includes, by mass percentage, 90% of silver-based conductive material, 3% of aluminum-based conductive material, 0.09% of titanium powder, 5% of glass material, 20% of organic carrier and 2% of slurry additive.

[0123] The method for preparing the electrode slurry provided in the embodiment of the present invention comprises the following steps:

[0124] The first step is to prepare glass material: 75% PbO, 20% B2O3, 2% SiO2 and 3% Fe2O3 are mixed by mass percentage, melted and quenched at high temperature, and then ground to obtain glass powder with a particle size of D50 = 0.5um ~ 3um, that is, glass material.

[0125] The second step is to prepare a premix: add titanium powder to the above glass material, stir evenly, and obtain a premix.

[0126] The third step is to prepare an organic carrier: by mass percentage, 40% of diethylene glycol butyl ether acetate, 10% of diisooctyl adipate, 5% of triethylene glycol diisooctanoate, 20% of pinene alcohol, and 6% of Thixatrol Max are mixed and stirred evenly, heated to 80°C for full activation, and then 15% of fumed alumina, 5% of ED120, and 2% of polyvinyl butyral resin are added, and stirring is continued. After the fumed silica is stirred evenly and the resin is fully dissolved, the organic carrier is obtained after standing and cooling.

[0127] The fourth step is to prepare the electrode slurry: the organic carrier, the premix, the silver-based conductive material, the aluminum-based conductive material and the slurry additive are evenly mixed, and the mixed silver slurry is placed on a three-roll mill for dispersion and grinding to obtain the electrode slurry.

[0128] The fifth step is to test the electrode slurry: print it on an N-type cell, sinter it at 730°C-780°C, and then use a Halm tester to test IV.

[0129] Comparative Example 1

[0130] Comparative Example 1 of the present invention uses commercially available silver-aluminum paste as comparative electrode paste, which does not contain the titanium powder and gas-phase inorganic nanomaterial of the present invention.

[0131] The present invention tests the performance of the electrode slurries prepared in Examples 1 to 4 and the electrode slurries of the comparative examples. First, by using silicon wafers with consistent square resistance, the prepared electrode slurry and the same main grid silver paste are respectively printed on the front and back fine grids and the front and back main grids of the battery by screen printing, and the back side is printed with the same electrode slurry once, and the battery cell is obtained by drying-sintering-cooling to room temperature. Secondly, the IV electrical performance test of the battery cell is performed using an IV tester. The test results of the embodiments and the comparative examples are as follows:

[0132] efficiency / % Opening voltage / V Short circuit current / A filling / % Series resistance / Ω Parallel resistance / Ω Example 1 23.965 0.7048 13.822 81.21 0.00156 371.2 Example 2 23.998 0.7056 13.840 81.11 0.00158 414.0 Example 3 24.024 0.7047 13.833 81.35 0.00146 366.7 Example 4 23.963 0.7055 13.827 81.08 0.00145 534.3 Comparative Example 1 23.810 0.7007 13.803 81.26 0.00142 163.4

[0133] As can be seen from the above table, the battery obtained by screen printing of the electrode slurry prepared in Examples 1 to 5 of the present invention has a higher battery opening voltage and a higher photoelectric conversion efficiency than that of Comparative Example 1. Therefore, the electrode slurry provided by the present invention can reduce the possibility of the anti-reflection layer being penetrated during the process of forming the electrode grid line on the battery cell by adding titanium powder, gas-phase inorganic nanomaterials and slurry additives to the electrode slurry, thereby avoiding the problem of emitter surface defects caused by excessive etching of the silicon substrate by the electrode slurry and the metal surface composite, thereby reducing leakage and improving the photoelectric conversion efficiency. .

[0134] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. An electrode slurry, characterized in that: include: Silver-based conductive material, glass material, organic carrier and titanium powder, wherein the glass material contains oxide and the glass material wraps the titanium powder; The organic carrier comprises a resin, an organic solvent, a surface dispersant and a gas-phase inorganic nanomaterial, the organic carrier is a liquid, the gas-phase inorganic nanomaterial is uniformly dispersed in the organic carrier, and the inorganic nanomaterial comprises at least one of gas-phase silicon dioxide, gas-phase aluminum oxide and gas-phase titanium dioxide; The preparation method of the electrode slurry comprises: The glass material is placed in a three-dimensional mixer and mixed evenly, and the evenly mixed glass material is placed in an alumina crucible for melting, the melted glass material is quenched, and then titanium powder is added so that the glass material evenly wraps the titanium powder to obtain a premix; Mixing resin, organic solvent and surface dispersant, and adding gas phase inorganic nanomaterial to mix, to obtain organic carrier; The organic vehicle, the premix, a silver-based conductive material, an aluminum-based conductive material and a slurry additive are mixed to obtain an electrode slurry.

2. The electrode slurry according to claim 1, characterized in that: In terms of mass percentage, the gas-phase inorganic nanomaterial accounts for 1% to 30% of the mass of the organic carrier.

3. The electrode slurry according to claim 1, characterized in that: The electrode slurry further includes an aluminum-based conductive material and a slurry additive.

4. The electrode slurry according to claim 3, characterized in that: The slurry additive includes at least one of silicon, magnesium, titanium, zinc, gallium powder, aluminum, tellurium, graphite powder and graphene powder.

5. The electrode slurry according to claim 3, characterized in that: The mass ratio of the glass material, the organic carrier, the titanium powder, the silver-based conductive material, the aluminum-based conductive material and the slurry additive is (1-7): (2-28): (0.05-1): (80-92): (0.5-4): (0.05-3).

6. The electrode slurry according to any one of claims 1 to 5, characterized in that: The glass material is at least one of PbO-B2O3-SiO2-Al2O3 system glass, PbO-B2O3-SiO2-Al2O3-ZnO system glass, V2O5-PbO system glass, Bi2O3-B2O3-SiO2 system glass, PbO-SiO2-Ti2O-ZnO system glass, and PbO-B2O3-SiO2-Fe2O3 system glass.

7. The electrode slurry according to any one of claims 3 to 5, characterized in that: The average particle size of the silver-based conductive material is 0.5 μm to 5 μm, and the particle size of the aluminum-based conductive material is in the range of 0.5 μm to 5 μm; The aluminum-based conductive material includes at least one of aluminum and aluminum alloy; The aluminum alloy includes at least one of an aluminum-silicon alloy, an aluminum-lead alloy, a boron-aluminum alloy, a gallium-aluminum alloy, and an indium-aluminum alloy.

8. A method for preparing an electrode slurry according to any one of claims 1 to 7, characterized in that: include: The glass material is placed in a three-dimensional mixer and mixed evenly, and the evenly mixed glass material is placed in an alumina crucible for melting, the melted glass material is quenched, and then titanium powder is added so that the glass material evenly wraps the titanium powder to obtain a premix; Mixing resin, organic solvent and surface dispersant, and adding gas phase inorganic nanomaterial to mix, to obtain organic carrier; The organic vehicle, the premix, a silver-based conductive material, an aluminum-based conductive material and a slurry additive are mixed to obtain an electrode slurry.

9. A photovoltaic cell, characterized in that: The photovoltaic cell has grid lines on its surface, and the material of the grid lines is the electrode slurry according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Conductive paste for front electrode of silicon crystal solar battery

    CN102637467A