A method for preparing nano titanium oxide and prepared nano titanium oxide

The preparation of nano-titanium oxide by combining starch materials with the sol-gel method solves the problem of high cost in existing technologies, realizes the industrial production of highly dispersible and high-purity nano-titanium oxide particles, and reduces equipment costs and environmental hazards.

CN115872443BActive Publication Date: 2024-11-15LIYANG TIANMU PILOT BATTERY MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111154342.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-29
Publication Date
2024-11-15
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Existing methods for preparing nano-titanium oxide are costly and difficult to apply industrially. In particular, the high cost of tetrabutyl titanate used in the liquid-phase method limits the industrial preparation of nano-titanium oxide.

Method used

The sol-gel method, using titanium-containing compounds and starch materials, is employed to prepare nano-titanium oxide particles by controlling temperature and atmosphere conditions, thus avoiding the use of acidic or alkaline substances, reducing raw material costs, and simplifying the process.

Benefits of technology

The prepared nano-titanium oxide particles have good dispersibility, high purity, stable process, and simple operation, which reduces equipment costs, reduces environmental hazards, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115872443B_ABST
    Figure CN115872443B_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of nano titanium oxide and the prepared nano titanium oxide. The preparation method comprises: adding water to dissolve a titanium-containing compound to prepare a solution with a concentration of 5% to 30%, adding starch material in proportion, stirring until uniform, placing in a preparation device, heating to 80°C to 120°C, keeping the temperature for 10min to 30min, so that starch molecules in the starch material are gelatinized to form a mesh-shaped colloid containing titanium ion solution, and then drying the obtained colloid at 60°C to 80°C to obtain a dry colloid; heating to 700°C to 1200°C at 1°C / min to 10°C / min in a nitrogen atmosphere, keeping the temperature for 1 hour to 10 hours, and obtaining a carbon matrix containing titanium nitride; heating the carbon matrix containing titanium nitride to 550°C to 900°C in an air atmosphere or an oxygen atmosphere, keeping the temperature for 1 hour to 12 hours to remove residual carbon in the carbon matrix containing titanium nitride, and oxidizing the titanium nitride to form nano titanium oxide particles, and then washing, filtering and drying the sample to obtain the nano titanium oxide particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to a method for preparing nano titanium oxide and the prepared nano titanium oxide. Background Art

[0002] Nano-titanium dioxide is a white powder and is widely used in photocatalysis, coatings, medicine, battery materials and other fields.

[0003] At present, the preparation methods of nano titanium oxide can be divided into physical method and chemical method. The physical method is mainly a crushing method, which has extremely high requirements for equipment, greatly increases the cost, and is difficult to be applied in industry. The chemical method mainly includes vapor deposition, liquid phase method and solid phase method. Among them, the sol-gel method (SG method for short) in the liquid phase method currently used is to use titanium-containing organic or inorganic salts as raw materials, and hydrolyze and polycondense in an organic medium by adding organic acid or inorganic acid as a hydrolysis inhibitor, so that the solution is subjected to a sol-gel process to obtain a gel, and the gel is heated (or frozen) dried, ground, and calcined to obtain the product. The powder obtained by this method has good dispersibility, high purity, easy reaction control, few side reactions, and simple process operation, but the cost of the raw materials used in this method is relatively high, and tetrabutyl titanate is more commonly used, which greatly limits the industrial preparation of nano titanium oxide. Summary of the invention

[0004] The embodiment of the present invention provides a method for preparing nano titanium oxide and the prepared nano titanium oxide, wherein nano titanium oxide particles are prepared by a sol-gel method, and have the advantages of good powder dispersibility, high purity, easy reaction control, stable process, and simple process operation. At the same time, the cost of raw materials is low, there is no acid, alkali or other substances in the preparation process, there is no need to consider the corrosion problem of production equipment, the environmental harm is reduced, and the existing production equipment can be used for batch rapid production, further reducing the equipment cost.

[0005] In a first aspect, an embodiment of the present invention provides a method for preparing nano titanium oxide, the method for preparing nano titanium oxide comprising:

[0006] The titanium-containing compound is dissolved in water to prepare a solution with a mass concentration of 5% to 30%, and the starch material is added in proportion and stirred until uniform to obtain a first solution;

[0007] The first solution is placed in a preparation device, heated to 80°C to 120°C, and kept warm for 10min to 30min, so that the starch molecules in the starch material are gelatinized to form a network-shaped colloid containing titanium ions, and then the obtained colloid is dried at 60°C to 80°C to obtain a dry colloid;

[0008] The dried colloid is heated to 700° C. to 1200° C. at a rate of 1° C. / min to 10° C. / min in a nitrogen atmosphere, and kept at this temperature for 1 to 10 hours to obtain a carbon matrix containing titanium nitride;

[0009] The carbon matrix containing titanium nitride is heated to 550°C to 900°C in an air atmosphere or an oxygen atmosphere, and kept warm for 1 to 10 hours to remove residual carbon in the carbon matrix containing titanium nitride, and the titanium nitride is oxidized to form nano titanium oxide particles, and then the sample is washed, filtered and dried to obtain the nano titanium oxide particles.

[0010] Preferably, the titanium-containing compound specifically includes any one or more of titanyl sulfate, titanium trichloride, titanium tetrachloride, and titanium iodide.

[0011] Preferably, the starch material specifically includes one or more combinations of corn starch, potato starch, tapioca starch or other starch raw materials that can form starch gelatinization colloid.

[0012] Preferably, in the first solution, the mass ratio of titanium ions in the titanium-containing compound to starch molecules in the starch material is 1:5 to 1:20.

[0013] Preferably, the stirring until uniform is specifically: stirring at a rotation speed of 100 r / min to 700 r / min until uniform.

[0014] In a second aspect, an embodiment of the present invention provides nano titanium oxide prepared by the method for preparing nano titanium oxide described in the first aspect.

[0015] Preferably, the particle size of the nano titanium oxide is between 5 nm and 500 nm.

[0016] The method for preparing nano titanium oxide provided by the embodiment of the present invention prepares nano titanium oxide particles by a sol-gel method, and the obtained product has the characteristics of good powder dispersibility and high purity; during the preparation process, the reaction is easy to control, the process is stable, the process operation is simple, and the raw material cost is low. There are no acid, alkali and other substances in the preparation process, and there is no need to consider the corrosion problem of production equipment, which reduces environmental hazards. In addition, currently available production equipment can be used for rapid batch production, further reducing equipment costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The technical solution of the embodiment of the present invention is further described in detail below through the drawings and examples.

[0018] Figure 1 A flow chart of a method for preparing nano titanium oxide provided by an embodiment of the present invention;

[0019] Figure 2A scanning electron microscope (SEM) image of nano titanium oxide provided in Example 1 of the present invention;

[0020] Figure 3 This is the X-ray diffraction (XRD) diagram of nano-titanium oxide provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0021] The present invention is further described below through the accompanying drawings and specific embodiments, but it should be understood that these embodiments are only used for more detailed description and should not be understood as limiting the present invention in any form, that is, they are not intended to limit the protection scope of the present invention.

[0022] The present invention proposes a method for preparing nano titanium oxide, the main steps of which are as follows: Figure 1 As shown, including:

[0023] Step 110, dissolving the titanium-containing compound in water to prepare a solution with a mass concentration of 5% to 30%, adding starch material in proportion, and stirring until uniform to obtain a first solution;

[0024] Specifically, the titanium-containing compound is preferably titanyl sulfate.

[0025] The starch material may specifically be a combination of one or more of corn starch, potato starch, tapioca starch or other starch raw materials that can form starch gelatinization colloid.

[0026] In the first solution, the mass ratio of titanium ions in the titanium-containing compound to starch molecules in the starch material is 1:5 to 1:20.

[0027] During the stirring process, the stirring speed is 100r / min to 700r / min, and the mixture is stirred thoroughly until uniform.

[0028] Step 120, placing the first solution in a preparation device, heating it to 80° C. to 120° C., and keeping it warm for 10 min to 30 min, so that the starch molecules in the starch material are gelatinized to form a network-shaped colloid containing the titanium ion solution, and then drying the obtained colloid at 60° C. to 80° C. to obtain a dry colloid;

[0029] Specifically, the preparation device can adopt existing equipment, such as a vermicelli machine.

[0030] In the implementation process of the present invention, the screw conveying time of the vermicelli machine is 10 minutes to 30 minutes, and the heating temperature ranges from 80°C to 120°C.

[0031] Step 130, heating the dried colloid to 700°C to 1200°C at 1°C / min to 10°C / min in a nitrogen atmosphere, and keeping the temperature for 1 hour to 10 hours to obtain a carbon matrix containing titanium nitride;

[0032] Step 140, heating the carbon matrix containing titanium nitride to 550°C to 900°C in an air atmosphere or an oxygen atmosphere, and keeping the temperature for 1 to 10 hours to remove residual carbon in the carbon matrix containing titanium nitride, and oxidize titanium nitride to form nano titanium oxide particles, and then wash, filter and dry the sample to obtain nano titanium oxide particles.

[0033] Specifically, in an air atmosphere or an oxygen atmosphere at 550°C to 900°C, carbon oxides are generated through an oxidation reaction of carbon to remove residual carbon in a carbon matrix containing titanium nitride. At the same time, at this reaction temperature, under the oxidizing action of oxygen, the chemical bonds in titanium oxide are broken, and titanium and oxygen are combined to form titanium oxide, so that nano titanium oxide particles can be finally obtained.

[0034] The particle size of the prepared nano titanium oxide is between 5nm and 500nm.

[0035] In order to better understand the technical solution provided by the present invention, the specific process of preparing nano titanium oxide by using the method provided by the above embodiment of the present invention is described below with multiple specific examples.

[0036] Example 1

[0037] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0038] Step 1: Take 200g of titanium oxysulfate and add 466ml of water to dissolve it to prepare a 30% solution, add 1200g of corn starch, and stir it at a speed of 100r / min until it is uniform.

[0039] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 80°C, and keep it warm for 30 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 60°C to obtain a dry colloid.

[0040] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 700°C at a rate of 1°C / min and kept at that temperature for 10 hours to obtain a carbon matrix containing titanium nitride.

[0041] Step 4: Heat the carbon matrix containing titanium nitride obtained in step 3 to 550° C. in an air atmosphere and keep it warm for 10 hours to remove residual carbon in the sample and oxidize titanium nitride nanoparticles to form nano-titanium oxide particles. Wash, filter and dry the sample to obtain nano-titanium oxide particles.

[0042] Figure 2 This is a scanning electron microscope (SEM) image of nano titanium oxide provided in Example 1 of the present invention, and the particle size is all at the nanometer level; Figure 3This is an X-ray diffraction (XRD) diagram of the nano-titanium oxide provided in Example 1 of the present invention. The XRD diagram shows that the nano-titanium oxide includes two crystal forms, rutile and anatase.

[0043] Example 2

[0044] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0045] Step 1: Take 200g of titanium oxysulfate and add 3800ml of water to dissolve it to prepare a 5% solution, add 300g of corn starch, and stir it at 700r / min until it is uniform.

[0046] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 120°C, and keep it warm for 10 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 80°C to obtain a dry colloid.

[0047] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 1200°C at a rate of 10°C / min and kept at that temperature for 1 hour to obtain a carbon matrix containing titanium nitride.

[0048] Step 4: Heat the carbon matrix containing titanium nitride obtained in step 3 to 550° C. in an air atmosphere and keep it warm for 1 hour to remove residual carbon in the sample and oxidize titanium nitride nanoparticles to form nano-titanium oxide particles. Wash, filter and dry the sample to obtain the nano-titanium oxide particles.

[0049] Example 3

[0050] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0051] Step 1: Take 200g of titanium oxysulfate and add 800ml of water to dissolve it to prepare a 20% solution, add 1000g of cassava starch, and stir it at a speed of 500r / min until it is uniform.

[0052] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 100°C, and keep it warm for 20 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 70°C to obtain a dry colloid.

[0053] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 1000°C at a rate of 3°C / min and kept at that temperature for 5 hours to obtain a carbon matrix containing titanium nitride.

[0054] Step 4: Heat the carbon matrix containing titanium nitride obtained in step 3 to 800° C. in an air atmosphere and keep it warm for 5 hours to remove residual carbon in the sample and oxidize titanium nitride nanoparticles to form nano-titanium oxide particles. Wash, filter and dry the sample to obtain the nano-titanium oxide particles.

[0055] Example 4

[0056] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0057] Step 1: Take 200g of titanium oxysulfate and add 800ml of water to dissolve to prepare a 20% solution, add 1000g of wheat starch, and stir at 500r / min until it is uniform.

[0058] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 100°C, and keep it warm for 20 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 80°C to obtain a dry colloid.

[0059] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 1100°C at a rate of 5°C / min and kept at that temperature for 5 hours to obtain a carbon matrix containing titanium nitride.

[0060] Step 4: Heat the carbon matrix containing titanium nitride obtained in step 3 to 700° C. in an oxygen atmosphere and keep it warm for 8 hours to remove residual carbon in the sample and oxidize titanium nitride nanoparticles to form nano-titanium oxide particles. Wash, filter and dry the sample to obtain the nano-titanium oxide particles.

[0061] Example 5

[0062] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0063] Step 1: Take 200g of titanium oxysulfate and add 1400ml of water to dissolve to prepare a solution with a concentration of 14.3%, add 800g of wheat starch, and stir at a speed of 500r / min until it is uniform.

[0064] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 110°C, and keep it warm for 30 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 80°C to obtain a dry colloid.

[0065] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 1100°C at 4°C / min in an ambient temperature and kept at that temperature for 5 hours to obtain a carbon matrix containing titanium nitride.

[0066] Step 4: The carbon matrix containing titanium nitride obtained in step 3 is heated to 700° C. in an air atmosphere, kept warm for 8 hours, and titanium nitride nanoparticles are oxidized to form nano-titanium oxide particles. The sample is washed, filtered, and dried to obtain the nano-titanium oxide particles.

[0067] Example 6

[0068] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0069] Step 1: Take 200g of titanium oxysulfate and add 800ml of water to dissolve it to prepare a 20% solution, add 800g of wheat starch, and stir at 200r / min until it is uniform.

[0070] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 90°C, and keep it warm for 30 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 80°C to obtain a dry colloid.

[0071] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 1150°C at a rate of 5°C / min and kept at that temperature for 8 hours to obtain a carbon matrix containing titanium nitride.

[0072] Step 4: Heat the carbon matrix containing titanium nitride obtained in step 3 to 850° C. in an air atmosphere and keep it warm for 8 hours to remove residual carbon in the sample and oxidize titanium nitride nanoparticles to form nano-titanium oxide particles. Wash, filter and dry the sample to obtain the nano-titanium oxide particles.

[0073] Example 7

[0074] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0075] Step 1: Take 200g of titanium oxysulfate and add 800ml of water to dissolve to prepare a 20% solution, add 1000g of pea starch, and stir at 400r / min until it is uniform.

[0076] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 115°C, and keep it warm for 10 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 80°C to obtain a dry colloid.

[0077] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 1100°C at a rate of 5°C / min and kept at that temperature for 5 hours to obtain a carbon matrix containing titanium nitride.

[0078] Step 4: Heat the carbon matrix containing titanium nitride obtained in step 3 to 950° C. in an air atmosphere and keep it warm for 5 hours to remove residual carbon in the sample and oxidize titanium nitride nanoparticles to form nano-titanium oxide particles. Wash, filter and dry the sample to obtain the nano-titanium oxide particles.

[0079] Example 8

[0080] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0081] Step 1: Take 200g of titanium oxysulfate and add 800ml of water to dissolve to prepare a 20% solution, add 600g of pea starch, and stir at 500r / min until it is uniform.

[0082] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 100°C, and keep it warm for 30 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 80°C to obtain a dry colloid.

[0083] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 1100°C at a rate of 5°C / min and kept at that temperature for 5 hours to obtain a carbon matrix containing titanium nitride.

[0084] Step 4: Heat the carbon matrix containing titanium nitride obtained in step 3 to 600° C. in an air atmosphere and keep it warm for 9 hours to remove residual carbon in the sample and oxidize titanium nitride nanoparticles to form nano-titanium oxide particles. Wash, filter and dry the sample to obtain the nano-titanium oxide particles.

[0085] Example 9

[0086] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0087] Step 1: Take 200g of titanium oxysulfate and add 800ml of water to dissolve to prepare a 20% solution, add 1000g of wheat starch, and stir at 500r / min until it is uniform.

[0088] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 120°C, and keep it warm for 10 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 80°C to obtain a dry colloid.

[0089] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 1100° C. at a rate of 7° C. / min and kept at that temperature for 5 hours to obtain a carbon matrix containing titanium nitride.

[0090] Step 4: Heat the carbon matrix containing titanium nitride obtained in step 3 to 750° C. in an air atmosphere and keep it warm for 6 hours to remove residual carbon in the sample and oxidize titanium nitride nanoparticles to form nano-titanium oxide particles. Wash, filter and dry the sample to obtain the nano-titanium oxide particles.

[0091] Example 10

[0092] This embodiment provides a method for preparing nano titanium oxide, comprising:

[0093] Step 1: Take 200g of titanium oxysulfate and add 800ml of water to dissolve to prepare a 20% solution, add 1000g of pea starch, and stir at 500r / min until it is uniform.

[0094] Step 2: Put the solution stirred evenly in step 1 into a vermicelli machine, heat it to 120°C, and keep it warm for 15 minutes. The starch molecules are gelatinized in this process to form a network of colloid containing titanium ion solution. The obtained sample is completely dried at 80°C to obtain a dry colloid.

[0095] Step 3: Place the dry colloid obtained in step 2 under N 2 The temperature was raised to 950°C at a rate of 10°C / min and kept at that temperature for 5 hours to obtain a carbon matrix containing titanium nitride.

[0096] Step 4: The carbon matrix containing titanium nitride obtained in step 3 is heated to 900°C in an oxygen atmosphere and kept at this temperature for 2 hours to remove the residual carbon in the sample and oxidize the titanium nitride nanoparticles to form nano-titanium oxide particles. The sample is washed, filtered and dried to obtain the nano-titanium oxide particles.

[0097] The method for preparing nano titanium oxide provided by the embodiment of the present invention prepares nano titanium oxide particles by a sol-gel method, and the obtained product has the characteristics of good powder dispersibility and high purity; during the preparation process, the reaction is easy to control, the process is stable, the process operation is simple, and the raw material cost is low. There are no acid, alkali and other substances in the preparation process, and there is no need to consider the corrosion problem of production equipment, which reduces environmental hazards. In addition, currently available production equipment can be used for rapid batch production, further reducing equipment costs.

[0098] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing nano titanium oxide, It is characterized in that The preparation method of the nano titanium oxide comprises: The titanium-containing compound is dissolved in water to prepare a solution with a mass concentration of 5% to 30%, and a starch material that can form a starch gelatinized colloid is added in proportion, and stirred until uniform to obtain a first solution; The first solution is placed in a preparation device, heated to 80°C to 120°C, and kept warm for 10min to 30min, so that the starch molecules in the starch material are gelatinized to form a network-shaped colloid containing titanium ions, and then the obtained colloid is dried at 60°C to 80°C to obtain a dry colloid; The dried colloid is heated to 700° C. to 1200° C. at a rate of 1° C. / min to 10° C. / min in a nitrogen atmosphere, and kept at this temperature for 1 to 10 hours to obtain a carbon matrix containing titanium nitride; The carbon matrix containing titanium nitride is heated to 550°C to 900°C in an air atmosphere or an oxygen atmosphere, and kept warm for 1 to 10 hours to remove residual carbon in the carbon matrix containing titanium nitride, and the titanium nitride is oxidized to form nano titanium oxide particles, and then the sample is washed, filtered and dried to obtain the nano titanium oxide particles.

2. The preparation method according to claim 1, It is characterized in that The titanium-containing compound specifically includes any one or more of titanyl sulfate, titanium trichloride, titanium tetrachloride, and titanium iodide.

3. The preparation method according to claim 1, It is characterized in that The starch material specifically includes one or more combinations of corn starch, potato starch, tapioca starch or other starch raw materials that can form starch gelatinization colloid.

4. The preparation method according to claim 1, It is characterized in that In the first solution, the mass ratio of titanium ions in the titanium-containing compound to starch molecules in the starch material is 1:5 to 1:

20.

5. The preparation method according to claim 1, It is characterized in that The stirring until uniform is specifically: stirring at a speed of 100 r / min to 700 r / min until uniform.