A metal lithium composite negative electrode and its preparation method and application

CN115911328BActive Publication Date: 2024-11-26INST OF ELECTRONICS ENG CHINA ACAD OF ENG PHYSICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211521357.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-11-26
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

然而,LiB合金中高的比容量往往对应低的热稳定性(液态金属锂溢流特性)

Benefits of technology

[0019] 1. A skeleton material is added to the metallic lithium composite negative electrode in the present invention. The skeleton material is evenly distributed in the composite negative electrode, which not only makes the obtained metallic lithium negative electrode more stable, but also extends the operating temperature of the metallic lithium negative electrode to 200-600°C. ; Moreover, during the working process, the skeleton material relies on capillary action to inhibit the free flow of liquid metal lithium in the composite material, which can effectively avoid the overflow of metal lithium in the composite negative electrode, and greatly improve the safety performance of the composite negative electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003973934270000011
    Figure HDA0003973934270000011
  • Figure HDA0003973934270000012
    Figure HDA0003973934270000012
  • Figure HDA0003973934270000021
    Figure HDA0003973934270000021
Patent Text Reader

Abstract

The present invention discloses a metal lithium composite negative electrode and a preparation method and application thereof. The metal lithium composite negative electrode comprises a skeleton material and metal lithium, wherein the skeleton material is LiC a , Li b Si c and Li d Al e At least one of; in order to improve the performance of the composite negative electrode, an auxiliary agent may also be added thereto, the auxiliary agent being at least one of Mg powder, Zn powder, Cu powder, Ag powder, Sn powder, Au powder, Ti powder and Mo powder. During preparation, the metallic lithium is first melted, and then the skeleton material and the auxiliary agent are added to the molten metallic lithium, and after a period of reaction, the metal is rolled, and then pressed into sheets or crushed into powder. The composite negative electrode prepared by the method of the present invention has both a high specific capacity and good safety performance, and can well meet the use requirements of thermal batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a metal lithium composite negative electrode and a preparation method and application thereof. Background Art

[0002] Thermal batteries have long storage time (storage time can reach 20 years), are maintenance-free, and have strong high current output capability (pulse current density can reach 10A cm -2 ), wide operating temperature range (-60℃~100℃), high reliability and other advantages are widely used in national defense, military and civilian fields. At present, lightweight and miniaturization are a major development trend of thermal batteries, and the development of high specific capacity thermal battery electrode materials has become a research hotspot.

[0003] In existing thermal battery products, liquid metal lithium composite materials are a kind of negative electrode materials that are used more frequently. By compounding metal lithium with porous skeleton materials, the capillary action of the skeleton materials is used to bind metal lithium in the electrode. Even at a temperature higher than the melting point of metal lithium, the composite negative electrode can work normally without liquid metal lithium overflow. Common skeleton materials used to bind metal lithium include Li7B6, carbon nanotubes, carbon fibers, graphene, Fe powder, Ni powder, etc. However, liquid metal lithium composite negative electrodes prepared using these skeleton materials often face the contradiction between specific capacity and safety. Taking LiB alloy as an example, by regulating the ratio of lithium and boron elements in the synthesis process of LiB alloy, a LiB alloy with a lithium content of 55-65wt% can be prepared, and the corresponding specific capacity is about 800-1500mAh / g. However, the high specific capacity in LiB alloy often corresponds to low thermal stability (liquid metal lithium overflow characteristics). Through analysis, it can be found that the improvement of the specific capacity of LiB alloy is usually achieved by increasing the metal lithium content inside the alloy, and the increase in the metal lithium content is the fundamental problem that leads to the reduction of the safety of LiB alloy. Summary of the invention

[0004] In view of the above-mentioned prior art, the present invention provides a metal lithium composite negative electrode and a preparation method and application thereof, so as to achieve the purpose of making the negative electrode of a thermal battery have both high specific capacity and good safety performance.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a metal lithium composite negative electrode, comprising the following components in mass percentage:

[0006] 30-95% skeleton material and 5-70% lithium metal; the skeleton material is LiC a , Li b Si c and Li d Al eAt least one of; wherein, 1 <a≤24;1<b≤25,1<c≤25;1<d≤10,1<e≤10。

[0007] Based on the above technical solution, the present invention can also be improved as follows.

[0008] Furthermore, the framework material is LiC6, Li 22 Si5 or LiAl.

[0009] Furthermore, the skeleton material is in granular, linear or three-dimensional network form; the particle size of the granular skeleton material is 1nm to 100μm; the length of the linear skeleton material is 100nm to 500μm and the diameter is 1nm to 100μm; the pore size of the three-dimensional network skeleton material is 50nm to 500μm.

[0010] Furthermore, the metal lithium composite negative electrode also includes an auxiliary agent, which is at least one of Mg powder, Zn powder, Cu powder, Ag powder, Sn powder, Au powder, Ti powder and Mo powder.

[0011] Furthermore, the additive accounts for 0.2wt% to 10wt% of the total mass of the framework material and the metallic lithium.

[0012] Furthermore, the particle size of the auxiliary agent is 0.5 to 50 μm.

[0013] The present invention also provides a method for preparing a metal lithium composite negative electrode, the preparation method comprising the following steps:

[0014] S1: In an inert gas environment, the temperature of the metallic lithium is raised to 200-500°C at a heating rate of 5-20°C / min; then, the framework material and the additive are added to the molten metallic lithium in batches under a stirring condition of 50-120r / min, and after stirring for 0.5-2h, the stirring speed is adjusted to 15-25r / min, and the reaction materials are cooled under stirring;

[0015] S2: After the reaction materials are cooled to below 100°C, they are rolled in an inert gas environment until the porosity is less than 40%;

[0016] S3: Pressing the rolled material into a sheet with a thickness of 50 to 1000 μm, or crushing it into particles with a particle size of 10 to 100 μm.

[0017] The present invention also provides a thermal battery, which is prepared using the above-mentioned metal lithium composite negative electrode as the negative electrode, a binary electrolyte (LiCl-KCl, etc.), a ternary all-lithium electrolyte (LiF-LiCl-LiBr) or a ternary low-melting point electrolyte (LiCl-LiBr-KBr or LiBr-KBr-LiF molten salt electrolyte) as the electrolyte, and at least one of FeCoS2, FeS2 and CoS2 as the positive electrode.

[0018] The beneficial effects of the present invention are:

[0019] 1. The metal lithium composite negative electrode of the present invention is added with a skeleton material, and the skeleton material is evenly distributed in the composite negative electrode, which can not only make the obtained metal lithium negative electrode more stable, so as to extend the working temperature of the metal lithium negative electrode to 200-600°C; but also in the working process, the skeleton material relies on capillary action to inhibit the free flow of liquid metal lithium in the composite material, which can effectively avoid the overflow of metal lithium in the composite negative electrode, and the safety performance of the composite negative electrode is greatly improved.

[0020] 2. The metal lithium composite negative electrode of the present invention is LiC a , Li b Si c , Li d Al e As the skeleton material of the composite negative electrode, the skeleton material itself includes Li. Even if the content of metallic lithium in the composite negative electrode is reduced, the final composite negative electrode still has a high specific capacity and can meet the use requirements of the thermal battery.

[0021] 3. The present invention can also add auxiliary agents when preparing the composite negative electrode. The addition of auxiliary agents helps to improve the adsorption effect of the skeleton material on liquid metal lithium, which can not only better prevent the overflow of molten metal lithium, but also make the skeleton material more evenly distributed in the composite negative electrode, thereby improving the performance of the negative electrode material.

[0022] 4. The skeleton material used in the application has good high-temperature stability, which can effectively avoid the problem of unsatisfactory product uniformity and consistency caused by intense heat release when using skeleton materials such as LiB to prepare composite negative electrodes. The final composite negative electrode has good uniformity and consistency, which helps to improve the performance consistency of thermal batteries.

[0023] 5. The existing thermal battery liquid metal lithium composite negative electrode has a high raw material price (such as metal boron powder) and a complex preparation process, resulting in a high overall price of thermal batteries; while the raw materials for the composite negative electrode of the present invention are low-priced and the preparation process is simple, which helps to reduce the cost of existing thermal batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1This is a comparison chart of thermal stability between sample A and sample C;

[0025] Figure 2 The discharge capacity comparison diagram of sample B and sample D;

[0026] Figure 3 This is a comparison chart of thermal stability between sample A and sample E;

[0027] Figure 4 The discharge capacity comparison diagram of sample B and sample F;

[0028] Figure 5 This is a comparison chart of the thermal stability of sample G and sample I;

[0029] Figure 6 The discharge capacity comparison chart of sample H and sample J. DETAILED DESCRIPTION

[0030] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0031] Example 1

[0032] A lithium metal composite negative electrode (Li 22 Si5-Li), including the following components in percentage by weight:

[0033] 30% skeleton material and 70% lithium metal; wherein the skeleton material is Li 22 Si5.

[0034] The metal lithium composite negative electrode in this embodiment is prepared by the following steps:

[0035] (1) In a high-purity argon (purity>99.99%) glove box, 70 g of high-purity metallic lithium (purity>99.9%) was placed in a stainless steel melting furnace, heated to 400° C. at a heating rate of 5° C. / min, and then kept at a constant temperature;

[0036] (2) 30 g of Li with a particle size of 1 μm was stirred. 22 Si5 powder was added into molten lithium in three times, with a stirring speed of 100 r / min;

[0037] (3)Li 22 After all Si5 powder is added, continue stirring and reacting for 1 hour; then stop heating and cool with the furnace, and maintain stirring during the cooling process at a stirring speed of 20r / min;

[0038] (4) When the temperature of the composite material is cooled to below 100° C., the composite material is taken out and repeatedly rolled using a rolling mill under nitrogen protection to reduce the porosity of the material to less than 40%;

[0039] (5) The composite material was pressed into a sheet with a thickness of 200 μm using a roller press, and then punched into a disc with a diameter of 32 mm to obtain a metal lithium composite negative electrode (Li 22 Si5-Li), sample number A.

[0040] The metal lithium composite negative electrode numbered A is combined with the binary molten salt electrolyte LiCl-KCl and FeCoS2 positive electrode, and pressed into shape to produce a single thermal battery, sample numbered B.

[0041] Example 2

[0042] A lithium metal composite negative electrode (Li 22 Si5-Li), including the following components in percentage by weight:

[0043] Framework material 28.5%, metallic lithium 66.7% and additives 4.8%; among which, the framework material is Li 22 Si5; the auxiliary agent is Mg powder.

[0044] The metal lithium composite negative electrode in this embodiment is prepared by the following steps:

[0045] (1) In a high-purity argon (purity>99.99%) glove box, 70 g of high-purity metallic lithium (purity>99.9%) was placed in a stainless steel melting furnace, heated to 400° C. at a heating rate of 5° C. / min, and then kept at a constant temperature;

[0046] (2) 30 g of Li with a particle size of 1 μm was stirred. 22 Si5 powder and 5 g of Mg powder with a particle size of 1 μm were added to the molten lithium metal three times at a stirring speed of 100 r / min;

[0047] (3)Li 22 After all Si5 and Mg powders are added, continue stirring and reacting for 1 hour; then stop heating and cool with the furnace, and maintain stirring during the cooling process at a stirring speed of 20r / min;

[0048] (4) When the temperature of the composite material is cooled to below 100° C., the composite material is taken out and repeatedly rolled using a rolling mill under nitrogen protection to reduce the porosity of the material to less than 40%;

[0049] (5) The composite material was pressed into a sheet with a thickness of 200 μm using a roller press, and then punched into a disc with a diameter of 32 mm to obtain a metal lithium composite negative electrode (Li 22 Si5-Li), sample number E.

[0050] The metal lithium composite negative electrode numbered E is combined with the binary molten salt electrolyte LiCl-KCl and FeCoS2 positive electrode, and pressed into shape to produce a single thermal battery, sample numbered F.

[0051] Example 3

[0052] A metal lithium composite negative electrode (LiC6-Li), comprising the following components in percentage by mass:

[0053] 40% skeleton material and 60% metallic lithium; wherein the skeleton material is LiC6.

[0054] The metal lithium composite negative electrode in this embodiment is prepared by the following steps:

[0055] (1) In a high-purity argon (purity>99.99%) glove box, 60 g of high-purity metallic lithium (purity>99.9%) was placed in a stainless steel melting furnace, heated to 300° C. at a heating rate of 5° C. / min, and then kept at a constant temperature;

[0056] (2) 40 g of LiC6 powder with a particle size of 2 μm was added to the molten lithium metal in three times under stirring conditions at a stirring speed of 100 r / min;

[0057] (3) After all the LiC6 powder is added, continue stirring and react for 1 hour; then stop heating and cool with the furnace. Keep stirring during the cooling process at a stirring speed of 20 r / min;

[0058] (4) When the temperature of the composite material is cooled to below 100° C., the composite material is taken out and repeatedly rolled using a rolling mill under nitrogen protection to reduce the porosity of the material to less than 40%;

[0059] (5) The composite material was pressed into a sheet with a thickness of 200 μm using a roller press, and then punched into a disc with a diameter of 32 mm to obtain a metallic lithium composite negative electrode (LiC6-Li), sample number G.

[0060] The metal lithium composite negative electrode numbered G is combined with the binary molten salt electrolyte LiCl-KCl and FeCoS2 positive electrode, and pressed into shape to produce a single thermal battery, sample numbered H.

[0061] Example 4

[0062] A lithium metal composite negative electrode (LiAl-Li) comprises the following components in percentage by mass:

[0063] 50% skeleton material and 50% metallic lithium; wherein the skeleton material is LiAl.

[0064] The metal lithium composite negative electrode in this embodiment is prepared by the following steps:

[0065] (1) In a high-purity argon (purity>99.99%) glove box, 50 g of high-purity metallic lithium (purity>99.9%) was placed in a stainless steel melting furnace, heated to 400° C. at a heating rate of 10° C. / min, and then the temperature was kept constant;

[0066] (2) adding 50 g of LiAl powder with a particle size of 50 nm into molten lithium in three times under stirring conditions at a stirring speed of 120 r / min;

[0067] (3) After all the LiAl powder is added, continue stirring and react for 1 hour; then stop heating and cool with the furnace. Keep stirring during the cooling process at a stirring speed of 15 r / min;

[0068] (4) When the temperature of the composite material is cooled to below 100° C., the composite material is taken out and repeatedly rolled using a rolling mill under nitrogen protection to reduce the porosity of the material to less than 40%;

[0069] (5) The rolled material is crushed into particles with a particle size of 50 μm using a crusher.

[0070] Example 5

[0071] A lithium metal composite negative electrode (Li 22 Si5-Li), compared with Example 1, the skeleton material is replaced with linear Li 22 Si5 (length: 10 μm, diameter: 100 nm), other operations are the same as in Example 1.

[0072] Example 6

[0073] A lithium metal composite negative electrode (Li 22 Si5-Li), compared with Example 1, the skeleton material is replaced by a three-dimensional network of Li 22 Si5 (outer dimensions are 10 μm, inner pore diameter is 100 nm to 500 nm), and the rest of the operations are the same as in Example 1.

[0074] Example 7

[0075] A lithium metal composite negative electrode (Li 12 Compared with Example 1, the framework material is replaced with powdered Li with a particle size of 500 nm. 12 Si7, the remaining operations are the same as those in Example 1.

[0076] Example 8

[0077] A metal lithium composite negative electrode (LiC-Li), compared with Example 1, the skeleton material is replaced by powdered LiC with a particle size of 10 μm, and the rest of the operations are the same as Example 1.

[0078] Example 9

[0079] A lithium metal composite negative electrode (Li 22Si5-Li), compared with Example 2, the auxiliary agent is replaced with Zn powder (particle size is 10μm), and the mass proportion of Zn powder is adjusted to 5wt% of the total mass of the skeleton material and metallic lithium, and the rest of the operations are the same as Example 2.

[0080] Example 10

[0081] A lithium metal composite negative electrode (Li 22 Si5-Li), compared with Example 2, the auxiliary agent is replaced with Cu powder (particle size is 0.5μm), and the mass proportion of Cu powder is adjusted to 10wt% of the total mass of the skeleton material and metallic lithium, and the rest of the operations are the same as Example 2.

[0082] Embodiment 11

[0083] A lithium metal composite negative electrode (Li 22 Si5-Li), compared with Example 2, the auxiliary agent is replaced with Ag powder (particle size is 50μm), and the mass proportion of Ag powder is adjusted to 2wt% of the total mass of the skeleton material and metallic lithium, and the rest of the operations are the same as Example 2.

[0084] Example 12

[0085] A lithium metal composite negative electrode (Li 22 Compared with Example 2, the auxiliary agent is replaced by Sn powder (particle size is 5 μm), and the mass proportion of Sn powder is adjusted to 1wt% of the total mass of the skeleton material and metallic lithium. The rest of the operations are the same as Example 2.

[0086] Embodiment 13

[0087] A lithium metal composite negative electrode (Li 22 Si5-Li), compared with Example 2, the auxiliary agent is replaced with Au powder (particle size is 20 μm), and the mass proportion of Au powder is adjusted to 0.5wt% of the total mass of the skeleton material and metallic lithium, and the rest of the operations are the same as Example 2.

[0088] Embodiment 14

[0089] A lithium metal composite negative electrode (Li 22 Si5-Li), compared with Example 2, the auxiliary agent is replaced with Ti powder (particle size is 1 μm), and the mass proportion of Ti powder is adjusted to 5wt% of the total mass of the skeleton material and metallic lithium, and the rest of the operations are the same as Example 2.

[0090] Embodiment 15

[0091] A lithium metal composite negative electrode (Li 22Si5-Li), compared with Example 2, the auxiliary agent is replaced with Mo powder (particle size is 5 μm), and the mass proportion of Mo powder is adjusted to 2wt% of the total mass of the skeleton material and metallic lithium, and the rest of the operations are the same as Example 2.

[0092] Example 16

[0093] A lithium metal composite negative electrode (Li 22 Compared with Example 2, the positive electrode in the single thermal battery is replaced with FeS2, and the rest of the operations are the same as in Example 2.

[0094] Embodiment 17

[0095] A lithium metal composite negative electrode (Li 22 Compared with Example 2, the positive electrode in the single thermal battery is replaced with CoS2, and the rest of the operations are the same as in Example 2.

[0096] Embodiment 18

[0097] A lithium metal composite negative electrode (Li 22 Compared with Example 2, the electrolyte in the single thermal battery is replaced with LiF-LiCl-LiBr, and the rest of the operations are the same as in Example 2.

[0098] Embodiment 19

[0099] A lithium metal composite negative electrode (Li 22 Compared with Example 2, the electrolyte in the single thermal battery is replaced with LiCl-LiBr-KBr, and the rest of the operations are the same as in Example 2.

[0100] Comparative Example 1

[0101] A metal lithium composite negative electrode (Li7B6-Li), comprising the following components in percentage by mass:

[0102] 30% skeleton material and 70% metallic lithium; wherein the skeleton material is Li7B6.

[0103] The metal lithium composite negative electrode is prepared by the following steps:

[0104] (1) In a high-purity argon (purity>99.99%) glove box, 70 g of high-purity metallic lithium (purity>99.9%) was placed in a stainless steel melting furnace, heated to 400° C. at a heating rate of 5° C. / min, and then kept at a constant temperature;

[0105] (2) adding 30 g of Li7B6 powder with a particle size of 1 μm into molten lithium metal in three times under stirring conditions at a stirring speed of 100 r / min;

[0106] (3) After all the Li7B6 powder is added, continue stirring and react for 1 hour; then stop heating and cool with the furnace. Keep stirring during the cooling process at a speed of 20 r / min;

[0107] (4) When the temperature of the composite material is cooled to below 100° C., the composite material is taken out and repeatedly rolled using a rolling mill under nitrogen protection to reduce the porosity of the material to less than 40%;

[0108] (5) The composite material was pressed into a sheet with a thickness of 200 μm using a roller press, and then punched into a disc with a diameter of 32 mm to obtain a metallic lithium composite negative electrode (Li7B6-Li), sample number C.

[0109] The metal lithium composite negative electrode numbered C was combined with the binary molten salt electrolyte LiCl-KCl and FeCoS2 positive electrode, and pressed into shape to produce a single thermal battery, sample numbered D.

[0110] Comparative Example 2

[0111] A metal lithium composite negative electrode, comprising the following components in percentage by mass:

[0112] 40% skeleton material and 60% metallic lithium; wherein the skeleton material is carbon fiber.

[0113] The metal lithium composite negative electrode is prepared by the following steps:

[0114] (1) In a high-purity argon (purity>99.99%) glove box, 60 g of high-purity metallic lithium (purity>99.9%) was placed in a stainless steel melting furnace, heated to 300° C. at a heating rate of 5° C. / min, and then kept at a constant temperature;

[0115] (2) adding 40 g of carbon fiber with a diameter of 2 μm into molten lithium in three times under stirring conditions at a stirring speed of 100 r / min;

[0116] (3) After all the LiC6 powder is added, continue stirring and react for 1 hour; then stop heating and cool with the furnace. Keep stirring during the cooling process at a stirring speed of 20 r / min;

[0117] (4) When the temperature of the composite material is cooled to below 100° C., the composite material is taken out and repeatedly rolled using a rolling mill under nitrogen protection to reduce the porosity of the material to less than 40%;

[0118] (5) The composite material was pressed into a sheet with a thickness of 200 μm using a roller press, and then punched into a disc with a diameter of 32 mm to obtain a metallic lithium composite negative electrode (LiC6-Li), sample number I.

[0119] The metal lithium composite negative electrode numbered I was combined with the binary molten salt electrolyte LiCl-KCl and FeCoS2 positive electrode, and pressed into shape to produce a single thermal battery, sample numbered J.

[0120] Results Analysis

[0121] Since the performance of the metal lithium composite negative electrode obtained in Examples 5 to 7 is similar to the performance of the metal lithium composite negative electrode obtained in Example 1, the performance of the metal lithium composite negative electrode obtained in Examples 9 to 15 is similar to the performance of the metal lithium composite negative electrode obtained in Example 2, the performance of the thermal battery obtained in Examples 16 to 19 is similar to the performance of the thermal battery obtained in Example 2, and the performance of the metal lithium composite negative electrode obtained in Example 4 is similar to the performance of the metal lithium composite negative electrode obtained in Example 3, the performance of the composite negative electrode is described by taking the metal lithium composite negative electrode obtained in Examples 1 to 3 as an example.

[0122] Figure 1 To compare the thermal stability of sample A and sample C, the test method is to clamp the sample to be tested with two stainless steel sheets and place it under constant temperature and pressure conditions of 550℃ and 500N for 10 minutes. Figure 1 It can be seen that under the test conditions, no obvious metallic lithium overflow was found at the edge of sample A. In sharp contrast, obvious metallic lithium overflow marks appeared at the edge of sample C, indicating that the thermal stability of sample A is significantly better than that of sample C. Figure 2 The discharge performance comparison of sample B and sample D, the test conditions are 500℃, 0.1Acm -2 Constant current discharge. Figure 2 It can be seen that under this discharge condition, the discharge capacity of sample B reaches more than 3300 As / g, while the discharge capacity of sample D is only 2750 As / g. 22 Compared with Li7B6-Li negative electrode material, Si5-Li composite negative electrode not only has better thermal stability but also higher discharge specific capacity.

[0123] Figure 3 The thermal stability of sample A and sample E is compared. The test method is to clamp the sample to be tested with two stainless steel sheets and place it under constant temperature and pressure conditions of 600℃ and 500N for 10 minutes. Figure 3 It can be seen that under the test conditions, obvious metallic lithium overflow has begun to appear at the edge of sample A. In contrast, no obvious signs of metallic lithium overflow appear at the edge of sample E, indicating that the thermal stability of sample E is better than that of sample A, that is, the sample containing the additive has higher thermal stability. Figure 4 The discharge performance comparison of sample B and sample F, the test conditions are 500℃, 0.1Acm -2Constant current discharge. It can be seen from the figure that under this discharge condition, the discharge capacity of sample B reaches more than 3300As / g, while the discharge capacity of sample F is 3100As / g. This experiment illustrates that the Li 22 The Si5-Li composite anode has better thermal stability, but due to the addition of inactive Mg powder, the Li 22 The specific capacity of Si5-Li composite negative electrode is slightly lower than that of material without additives.

[0124] Figure 5 The thermal stability of sample G and sample I is compared. The test method is to clamp the sample to be tested with two stainless steel sheets and place it under constant temperature and pressure conditions of 500℃ and 500N for 10 minutes. Figure 5 It can be seen that under this test condition, there is no obvious metallic lithium overflow at the edge of sample G. In contrast, there are obvious signs of metallic lithium overflow at the edge of sample I, indicating that the thermal stability of sample G is better than that of sample I. In other words, the composite negative electrode material using a LiC6 skeleton has higher thermal stability than that using carbon fiber. Figure 6 The discharge performance comparison of sample H and sample J, the test conditions are 500℃, 0.1Acm -2 Constant current discharge. As can be seen from the figure, under this discharge condition, the discharge capacity of sample H is about 3000As / g, while sample J has a short circuit during the discharge process. The short circuit phenomenon of sample J during the discharge process well illustrates its poor thermal stability and the easy occurrence of metal lithium overflow in a high temperature working environment.

[0125] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing a metallic lithium composite negative electrode, characterized in that: The following steps are involved: S1: Heat metallic lithium to 200 - 500 °C at a heating rate of 5 - 20 °C / min in an inert gas environment; then, under stirring conditions of 50 - 120 r / min, add the skeleton material and the auxiliary agent to the molten metallic lithium in batches. After stirring and reacting for 0.5 - 2 h, adjust the stirring speed to 15 - 25 r / min, and cool the reaction material under stirring conditions; the skeleton material is LiC a , Li b Si c and Li d Al e at least one of them; where 1 < a ≤ 24; 1 < b ≤ 25, 1 < c ≤ 25; 1 < d ≤ 10, 1 < e ≤ 10; the auxiliary agent is at least one of Mg powder, Zn powder, Cu powder, Ag powder, Sn powder, Au powder, Ti powder and Mo powder; S2: After the reaction materials are cooled to below 100°C, they are rolled in an inert gas environment until the porosity is less than 40%; S3: Press the rolled material into a sheet with a thickness of 50-1000 μm, or crush it into particles with a particle size of 10-100 μm.

2. The method for preparing a metallic lithium composite negative electrode according to claim 1, characterized in that: The metal lithium composite negative electrode comprises the following components in percentage by mass: Skeleton material 30~95% and metallic lithium 5~70%.

3. The method for preparing a metallic lithium composite negative electrode according to claim 1, characterized in that: The framework material is LiC6, Li 22 Si5 or LiAl.

4. The method for preparing a metal lithium composite negative electrode according to claim 3, characterized in that: The skeleton material is in granular, linear or three-dimensional mesh form; the particle size of the granular skeleton material is 1nm~100μm; the length of the linear skeleton material is 100nm~500μm, and the diameter is 1nm~100μm; the pore size of the three-dimensional mesh skeleton material is 50nm~500μm.

5. The method for preparing a metal lithium composite negative electrode according to claim 4, characterized in that: The auxiliary agent accounts for 0.2wt% to 10wt% of the total mass of the framework material and the metallic lithium.

6. The method for preparing a metallic lithium composite negative electrode according to claim 4, characterized in that: The particle size of the auxiliary agent is 0.5-50 μm.

7. Use of the metal lithium composite negative electrode prepared by the method for preparing the metal lithium composite negative electrode according to any one of claims 1 to 6 in preparing a thermal battery.

8. The use according to claim 7, characterized in that: The negative electrode of the thermal battery is a metal lithium composite negative electrode, the positive electrode is at least one of FeCoS2, FeS2 and CoS2, and the electrolyte is a binary electrolyte, a ternary all-lithium electrolyte or a ternary low-melting-point electrolyte.

9. The use according to claim 8, characterized in that: The binary electrolyte is a binary molten salt electrolyte LiCl-KCl; the ternary all-lithium electrolyte is a LiF-LiCl-LiBr molten salt electrolyte, and the ternary low-melting-point electrolyte is a LiCl-LiBr-KBr or LiBr-KBr-LiF molten salt electrolyte.