Stainless steel for metal foil, stainless steel foil and method for producing the same

By adjusting the stainless steel composition and refining process, controlling the slag composition and stirring power, the surface defects and manufacturing deviations caused by hard inclusions in the general refining method were solved, and high-quality stainless steel foil production was achieved.

CN115917013BActive Publication Date: 2024-11-26NIPPON STEEL STAINLESS STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180012734.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-27
Filing Date
2021-02-24
Publication Date
2024-11-26
Estimated Expiration
2041-02-24

AI Technical Summary

Technical Problem

In stainless steel manufactured by existing general refining methods, it is difficult to avoid surface defects caused by hard inclusions and deviations in perforation and fatigue characteristics during manufacturing, especially the problems of MgO·Al2O3 or MnO·Al2O3·Cr2O3 inclusions.

Method used

By adjusting the composition of stainless steel and refining processes, controlling slag composition and stirring power, the formation of hard inclusions can be reduced. Specific measures include using Fe-Si alloys or metallic Si for deoxidation, adjusting the CaO/SiO2 ratio and Al2O3 content, and conducting thorough stirring of the molten steel to ensure that inclusions are refined during the rolling process.

Benefits of technology

It effectively reduces surface defects and perforation and fatigue characteristic deviations in stainless steel foil during manufacturing, improves the surface properties of stainless steel foil, and ensures a high-quality production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003781475200000091
    Figure BDA0003781475200000091
  • Figure BDA0003781475200000111
    Figure BDA0003781475200000111
  • Figure BDA0003781475200000121
    Figure BDA0003781475200000121
Patent Text Reader

Abstract

A stainless steel for metal foil having excellent surface properties, a stainless steel foil and a method for producing the same, wherein the stainless steel contains, by mass%, 0.0001% to 0.15% C, 0.30% to 2.0% Si, 0.1% to 15% Mn, 0.040% to 30% P, 5% to 30% Ni, 0.0001% to 0.01% S, 16% to 25% C. R, 5% or less Mo, 0.005% or less Al, 0.0030% or less Ca, 0.0010% or less Mg, 0.0010% or more and 0.0060% or less O, 0.0001% or more and 0.5% or less N, the remainder being Fe and unavoidable impurities, and the number of inclusions with a maximum equivalent circle diameter of 5 μm or more in a thickness of 0.010 mm or more and 0.2 mm or less is 0.5 pieces / mm 2 the following.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to stainless steel for metal foil used for electronic equipment parts and the like, stainless steel foil, and a method for producing the same. Background Art

[0002] Conventionally, methods for producing ultra-clean stainless steel are roughly divided into two methods: a method using a special melting / remelting method and a method using a general refining method.

[0003] In the case of a method using a special melting / remelting method, although a high cleanliness can be achieved, the productivity of the manufacturing method is extremely low and the manufacturing cost is also high, so it is not suitable for mass production purposes. Therefore, a general refining method is generally used. However, in the case of a general refining method, although mass production can be achieved at a relatively low cost, it is not technically easy to obtain a high cleanliness.

[0004] Therefore, it is desirable to achieve higher cleanliness while using a general refining process.

[0005] For example, Patent Document 1 describes a method in which, in a refining step, defects caused by Al 2 O 3 inclusions are suppressed by setting the basicity to 1.0 to 1.5 and the Al 2 O 3 concentration in the slag to 10% or less.

[0006] Patent Document 2 describes a method of suppressing MgO·Al 2 O 3 by setting the basicity to 2 to less than 5 and reducing the Al 2 O 3 concentration in the slag in the refining step.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent No. 3416858

[0010] Patent Document 2: Japanese Patent No. 6146908 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, in the method of Patent Document 1, since the upper limit of the Al2O3 concentration in the slag is high, large and hard MgO·Al2O3 inclusions with an equivalent circle diameter of 5 μm or more containing Al2O3 may be generated. When such inclusions are generated, since they are not extended during the rolling process, linear defects are not observed, which does not become a problem for the subject of Patent Document 1. However, as a material for stainless steel made into an extremely thin layer by customers, etc., it may be impossible to prevent the occurrence of surface defects.

[0013] In addition, in the method of Patent Document 2, there is a case where steel with a high oxygen concentration is produced due to insufficient deoxidation, and large and hard MnO·Al2O3·Cr2O3 inclusions with an equivalent circle diameter of 5 μm or more may be generated. When such inclusions are generated, it may be impossible to prevent the occurrence of surface defects as a material for stainless steel made into an extremely thin layer by a customer.

[0014] Thus, in stainless steel produced by the general refining method, there are hard inclusions mainly composed of MgO·Al2O3 or MnO·Al2O3·Cr2O3. These hard inclusions exhibit different deformation behavior from the base material due to the difference in hardness with the base material during grinding, thus causing deviations in perforation and fatigue properties during manufacturing. In addition, in the methods of Patent Documents 1 and 2, composition changes during heating, deformation, extension, and crushing of inclusions during rolling are not considered, and it may be impossible to prevent surface defects from occurring in extremely thin stainless steel formed into a foil shape.

[0015] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a stainless steel for metal foil having excellent surface properties, a stainless steel foil, and a method for producing the same.

[0016] Means for solving problems

[0017] The stainless steel for metal foil according to claim 1 contains C: 0.0001 mass % or more and 0.15 mass % or less, Si: 0.30 mass % or more and 2.0 mass % or less, Mn: 0.1 mass % or more and 15 mass % or less, P: 0.040 mass % or less, Ni: 5 mass % or more and 30 mass % or less, S: 0.0001 mass % or more and 0.01 mass % or less, Cr: 16 mass % or more and 25 mass % or less, Mo: 5 mass % or less, Al: 0.005 mass % or less, Ca: 0.0030 mass % or less, Mg: 0.0010 mass % or less, O: 0.0010 mass % or more and 0.0060 mass % or less, N: 0.0001 mass % or more and 0.5 mass % or less, the remainder is Fe and unavoidable impurities, and in a thickness of 0.010 mm or more and 0.2 mm or less, the number of inclusions with a maximum equivalent circle diameter of 5 μm or more is 0.5 pieces / mm 2 the following.

[0018] The stainless steel for metal foil described in Technical Solution 2 is a stainless steel for metal foil described in Technical Solution 1 that does not contain first inclusions with an equivalent circle diameter of 5 μm or more (whose average composition is MnO: 10 mass% or more, Cr2O3+Al2O3: 30 mass% or more, CaO: 10 mass% or less) and second inclusions with an equivalent circle diameter of 5 μm or more (whose average composition is MgO: 10 mass% or more, Al2O3: 20 mass% or more).

[0019] The stainless steel for metal foil described in Technical Solution 3 is the stainless steel for metal foil described in Technical Solution 1 or 2, which further contains at least any one of Cu: 0.1 mass% to 4.0 mass%, REM: 0.00001 mass% to 0.0030 mass%, B: 0.0001 mass% to 0.0050 mass%, Ti: 0.01 mass% to 0.50 mass%, Nb: 0.01 mass% to 0.50 mass%, V: 0.01 mass% to 1.00 mass%, W: 0.01 mass% to 1.00 mass%, Co: 0.01 mass% to 1.00 mass%, and Sn: 0.01 mass% to 1.00 mass%.

[0020] The stainless steel foil according to claim 4 has a thickness of 0.010 mm to 0.2 mm, and a composition comprising C: 0.0001 mass % to 0.15 mass %, Si: 0.30 mass % to 2.0 mass %, Mn: 0.1 mass % to 15 mass %, P: 0.040 mass % to 0.040 mass %, Ni: 5 mass % to 30 mass %, S: 0.0001 mass % to 0.01 mass %, Cr: 16 mass% or more and 25 mass% or less, Mo: 5 mass% or less, Al: 0.005 mass% or less, Ca: 0.0030 mass% or less, Mg: 0.0010 mass% or less, O: 0.0010 mass% or more and 0.0060 mass% or less, N: 0.0001 mass% or more and 0.5 mass% or less, the remainder is Fe and unavoidable impurities, and the maximum number of inclusions with an equivalent circle diameter of 5 μm or more is 0.5 pieces / mm 2 the following.

[0021] The stainless steel foil described in technical solution 5 is the stainless steel foil described in technical solution 4 and further contains at least any one of Cu: 0.1 mass% to 4.0 mass%, REM: 0.00001 mass% to 0.0030 mass%, B: 0.0001 mass% to 0.0050 mass%, Ti: 0.01 mass% to 0.50 mass%, Nb: 0.01 mass% to 0.50 mass%, V: 0.01 mass% to 1.00 mass%, W: 0.01 mass% to 1.00 mass%, Co: 0.01 mass% to 1.00 mass%, and Sn: 0.01 mass% to 1.00 mass%.

[0022] The method for manufacturing stainless steel for metal foil described in Technical Solution 6 is a method for manufacturing stainless steel for metal foil according to any one of Technical Solutions 1 to 3, which comprises a refining process using VOD or AOD for refining. In the refining process, Al and Al2O3 contained in the raw material or the ladle are adjusted, deoxidation is carried out using Fe-Si alloy or metal Si, and CaO or SiO2 is added, thereby making the slag composition, in terms of mass %, CaO / SiO2: greater than 1.1 and less than 1.7, Al2O3: less than 4.0 mass %, and MgO: less than 10.0 mass %, and further, after adding the refined slag raw material and the alloy raw material, the molten steel is stirred for more than 5 minutes at a stirring power of more than 50W / ton.

[0023] The method for manufacturing the stainless steel foil described in Technical Solution 7 is a method for manufacturing the stainless steel foil described in Technical Solution 4 or 5, which comprises a refining step of refining by VOD or AOD, in which the Al and Al2O3 contained in the raw material or the ladle are adjusted, deoxidation is performed using a Fe-Si alloy or metallic Si, and CaO or SiO2 is added, thereby making the slag composition in terms of mass % ratio of CaO / SiO2: greater than 1.1 and less than 1.7, Al2O3: less than 4.0 mass %, and MgO: less than 10.0 mass %, and further, after adding the refined slag raw material and the alloy raw material, the molten steel is stirred for more than 5 minutes at a stirring power of more than 50 W / ton.

[0024] Effects of the Invention

[0025] According to the present invention, it is possible to reduce the puncture during production and the variation in fatigue properties, and to achieve excellent surface properties. DETAILED DESCRIPTION

[0026] Hereinafter, one embodiment of the present invention will be described.

[0027] The stainless steel for metal foil of the present embodiment (hereinafter referred to as stainless steel) is an austenitic stainless steel for metal foil, and contains 0.0001 mass % to 0.15 mass % C (carbon), 0.30 mass % to 2.0 mass % Si (silicon), 0.1 mass % to 15 mass % Mn (manganese), 0.040 mass % to 15 mass % P (phosphorus), 5 mass % to 30 mass % Ni (nickel), 0.0001 mass % to 0.01 S (sulfur) of less than 16 mass %, Cr (chromium) of more than 16 mass % and less than 25 mass %, Mo (molybdenum) of less than 5 mass %, Al (aluminum) of less than 0.005 mass %, Ca (calcium) of less than 0.0030 mass %, Mg (magnesium) of less than 0.0010 mass %, O (oxygen) of more than 0.0010 mass % and less than 0.0060 mass %, N (nitrogen) of more than 0.0001 mass % and less than 0.5 mass %, and the remainder is composed of Fe (iron) and inevitable impurities. It should be noted that Cu (copper) of more than 0.1 mass % and less than 4.0 mass % and / or REM (rare earth element) of more than 0.00001 mass % and less than 0.0030 mass % can also be contained in stainless steel. In addition, stainless steel can also contain elements such as Sn (tin), Nb (niobium), Ti (titanium), Co (cobalt), V (vanadium), W (tungsten), and B (boron) in a specified amount.

[0028] The stainless steel foil of the present embodiment is manufactured through a predetermined manufacturing process described later so as to have a thickness of 0.010 mm or more and 0.2 mm or less.

[0029] In addition, regarding the stainless steel of the present embodiment, in order to prevent perforation and fatigue characteristics in the final foil product, the number density of hard inclusions with large equivalent circle diameters is suppressed. Specifically, the stainless steel of the present embodiment does not contain first inclusions with an equivalent circle diameter of 5 μm or more (in terms of mass ratio, its average composition is MnO: 10 mass% or more, Cr2O3+Al2O3: 30 mass% or more, CaO: 10 mass% or less) and second inclusions with an equivalent circle diameter of 5 μm or more (in terms of mass ratio, its average composition is MgO: 10 mass% or more, Al2O3: 20 mass% or more) in steel sheets (cast sheets) such as slabs before hot rolling. In addition, in the foil state, the number density of inclusions with a maximum equivalent circle diameter of 5 μm or more among the number of inclusions measured in any cross section of the stainless steel of the present embodiment is adjusted to 0.5 / mm 2The first inclusion and the second inclusion change their composition into hard MgO·Al2O3 or MnO·Al2O3·Cr2O3 inclusions by rolling the slab. When stainless steel is rolled from a slab, the surface area becomes larger, while the inclusions contained inside are exposed on the surface. Therefore, as long as it is rolled into a foil, the number of inclusions per unit area remains basically unchanged regardless of the observation position.

[0030] C is an austenite stabilizing element, and the hardness and strength of stainless steel are increased by containing C. On the other hand, when C is excessive, it reacts with Cr and Mn of the base material, and the corrosion resistance deteriorates. Therefore, the content of C is set to 0.0001 mass % or more and 0.15 mass % or less, preferably 0.1 mass % or less.

[0031] Si is an element necessary for deoxidation under low Al conditions. However, when the Si content is higher than 2.0 mass%, in addition to promoting the formation of hot rolling defects, the workability is also reduced. Therefore, the Si content is set to 0.30 mass% or more and 2.0 mass% or less, preferably 0.50 mass% or more and 1.0 mass% or less.

[0032] Mn is an element effective for deoxidation and is also an austenite stabilizing element. When the content of Mn is less than 0.1% by mass, the hot brittleness caused by the formation of FeS is promoted, which has an adverse effect on manufacturability. Therefore, the content of Mn is set to 0.1% by mass or more, preferably 0.5% by mass or more and 15% by mass or less.

[0033] P is an impurity in the steelmaking process. If the P content exceeds 0.050 mass%, hot brittleness decreases, so it is set to 0.040 mass% or less. The P content is preferably 0.030 mass% or less.

[0034] Ni is an element that improves the corrosion resistance of stainless steel and is also an austenite stabilizing element. The content of Ni is set to 5 mass % or more and 30 mass % or less.

[0035] S is an element that improves the melting property of stainless steel during welding. However, when the S content exceeds 0.01 mass%, sulfide inclusions are generated, and the corrosion resistance is reduced. Therefore, the S content is set to 0.0001 mass% or more and 0.01 mass% or less, preferably 0.005 mass% or less.

[0036] Cr is an element necessary to ensure the corrosion resistance of stainless steel. However, when the Cr content exceeds 25 mass%, the manufacture of stainless steel becomes difficult, and the content of Cr2O3 in inclusions increases, so MnO·Al2O3·Cr2O3 is easily generated. Therefore, the Cr content is set to 16 mass% or more and 25 mass% or less.

[0037] Cu is an element that improves the workability of stainless steel and is also an austenite stabilizing element. When the content of Cu is higher than 4.0 mass %, cracks in the casting sheet etc. are generated, which has a negative impact on manufacturability. In addition, Cu is an optional element, including the case of no addition. Therefore, the content of Cu is set to more than 0 mass % and less than 4.0 mass %, and when containing Cu, it is set to more than 0.1 mass % and less than 4.0 mass %.

[0038] Mo is an element that improves the corrosion resistance of stainless steel. However, when the content of Mo is higher than 5 mass%, it promotes the formation of σ phase and causes embrittlement of the base material, which is not preferred. Therefore, the content of Mo is set to 5 mass% or less, preferably 0.01 mass% or more and 3 mass% or less.

[0039] Al is an element sometimes added as a deoxidizing material to stainless steel produced by a general refining method, but in Si deoxidized steel such as the present invention, it is an element that is inevitably mixed due to the melting loss of impurities in the raw materials, refractory materials, etc. In addition, when the content of Al is higher than 0.005 mass%, large and hard MgO·Al2O3 and / or large and hard MnO·Al2O3·Cr2O3 are generated, resulting in deviations in perforation and fatigue properties during manufacturing. Therefore, the content of Al is set to 0.005 mass% or less, preferably 0.003 mass% or less.

[0040] Ca is an element that improves the hot workability of stainless steel. Ca can also be added in the form of Ca-Si alloy after refining of VOD or AOD described later. In the present embodiment, when the content of Ca is higher than 0.0030 mass%, the number of inclusions in the foil increases due to the generation of coarse slag-based inclusions in the cast sheet. Therefore, the content of Ca is set to 0.0030 mass% or less (excluding the case of no addition), preferably 0.0010 mass% or less.

[0041] Mg is an element effective for deoxidation, and is an element that is inevitably mixed into the Si deoxidized steel of the present invention due to the melting loss of impurities in the raw materials and refractory materials. However, when the content exceeds 0.0010 mass%, large and hard MgO·Al2O3 is generated, which leads to the deviation of the perforation and fatigue characteristics during the manufacturing process. Therefore, the content of Mg is set to 0.0010 mass% or less, preferably 0.0005 mass% or less.

[0042] When the content of O is less than 0.0010 mass%, large and hard MgO·Al2O3 is generated, which leads to puncture and fatigue property deviation during manufacturing. In addition, when the content of O is more than 0.0060 mass%, large and hard MnO·Al2O3·Cr2O3 is generated, which leads to puncture and fatigue property deviation during manufacturing. Therefore, the content of O is set to 0.0010 mass% or more and 0.0060 mass% or less, preferably 0.0020 mass% or more and 0.0050 mass% or less.

[0043] N is an element that improves the corrosion resistance of stainless steel and is also an austenite stabilizing element. When the content of Al is the above-mentioned low content, N does not generate inclusions, but when the content is higher than 0.5 mass%, bubbles are generated in the steel ingot, which has an adverse effect on the manufacturability of stainless steel. Therefore, the content of N is set to be greater than 0.0001 mass% and less than 0.5 mass%.

[0044] REM is an element that improves the hot workability of stainless steel. When the content of REM is higher than 0.0030 mass%, nozzle clogging occurs, which adversely affects the manufacturability of stainless steel. In addition, REM is an optional element, so it also includes the case where it is not added. Therefore, the content of REM is set to be greater than 0 mass% and less than 0.0030 mass%, and when REM is contained, it is set to be greater than 0.00001 mass% and less than 0.0030 mass%.

[0045] B, like Ca, is an element that improves the hot workability of stainless steel, and therefore may be added in an amount of 0.0050 mass % or less as necessary. When added, the content is preferably 0.0001 mass % or more and 0.0030 mass % or less.

[0046] Ti and Nb form precipitates with C or N, which are effective in preventing grain coarsening during heat treatment, and thus can be added in a range of 0.50 mass % or less. When added, the content is preferably 0.01 mass % or more and 0.30 mass % or less.

[0047] V, W, Co, and Sn are all elements that improve the corrosion resistance of stainless steel and can be added as needed. When added, the content of V is preferably 0.01% by mass to 1.00% by mass, W is preferably 0.01% by mass to 1.00% by mass, Co is preferably 0.01% by mass to 1.00% by mass, and Sn is preferably 0.01% by mass to 1.00% by mass.

[0048] Next, a method for producing the above-mentioned stainless steel will be described.

[0049] When the above-mentioned stainless steel is produced, raw materials are melted and refined, and the stainless steel having the components adjusted as described above is molten.

[0050] In the refining process, VOD or AOD is used, and LF may be performed after AOD.

[0051] In the present embodiment, in order to suppress the generation of slag-based inclusions generated during reduction in the refining process, the slag composition is controlled by making the reduced material highly purified and controlling the input amount, and the composition of inclusions in the stainless steel is controlled by specifying the deoxidizing element and O concentration in the metal.

[0052] That is, when MgO·Al2O3 and MnO·Al2O3·Cr2O3 are generated in the slag-based inclusions (CaO-SiO2-Al2O3-MgO-MnO-Cr2O3 system) mainly confirmed in the cast piece, the slag-based inclusions are extended and refined during rolling, while the hard MgO·Al2O3 and MnO·Al2O3·Cr2O3 remain as relatively large inclusions in the final foil product, resulting in puncture and fatigue properties being reduced during manufacturing. Therefore, in the present embodiment, the slag composition, deoxidizing elements and O concentration are adjusted to achieve a state in which MnO·Al2O3·Cr2O3 is easily generated (easy to control to become a fine inclusion in the foil state), and MnO·Al2O3·Cr2O3 is made fine.

[0053] In this embodiment, in the refining process, the Al and Al2O3 contained in the raw material or the ladle are adjusted to be removed within the range that does not hinder refining. In addition, a sufficient amount of Fe-Si alloy or metal Si is used for deoxidation, and CaO or SiO2 is added so that the O concentration in the steel becomes the above range. At this time, in order to ensure the fluidity of the slag, a predetermined amount of CaF2 may also be contained.

[0054] Thus, the composition of the refined slag is controlled to be, in mass %, CaO / SiO2: 1.1 or more and 1.7 or less, preferably 1.2 or more and 1.6 or less, Al2O3: 4.0 mass % or less, preferably 2.0 mass % or less, and MgO: 10.0 mass % or less, preferably 8.0 mass % or less. The slag composition is the value after VOD, or after AOD and LF. If CaO / SiO2 is higher than 1.7, the second inclusion is generated, and if CaO / SiO2 is lower than 1.1, the first inclusion is generated.

[0055] In addition, after the refining slag is added, the molten steel is stirred for more than 5 minutes with a stirring power of more than 50W / ton. If the stirring power is less than 50W / ton, the second inclusions with low density and high harmfulness will not fully float up, and thus become excessive. In addition, if the stirring holding time is less than 5 minutes, neither the first inclusions nor the second inclusions float up, and become excessive. When the stirring power is more than 150W / ton, it is possible to involve the slag present on the molten steel, and the second inclusions increase, so it is preferred to make the stirring power less than 150W / ton. There is no particular limit to the upper limit of the stirring holding time, but considering that the effect brought by the stirring is saturated and the load on the equipment and the manufacturing efficiency are reduced, it is preferred to make the stirring holding time less than 30 minutes. In addition to the method of gas blowing using VOD or LF, stirring can also be implemented by other methods such as mechanical mixing or electromagnetic stirring.

[0056] Then, after the refining step, the continuous casting step is performed to form a slab having a predetermined thickness.

[0057] As a result, stainless steel can be produced that does not contain first inclusions with an equivalent circle diameter of 5 μm or more (whose average composition is MnO: 10 mass % or more, Cr2O3+Al2O3: 30 mass % or more, CaO: 10 mass % or less) and second inclusions with an equivalent circle diameter of 5 μm or more (whose average composition is MgO: 10 mass % or more, Al2O3: 20 mass % or more).

[0058] Therefore, for this stainless steel, when a stainless steel foil having a thickness of 0.010 mm or more and 0.2 mm or less is manufactured through a hot rolling process, a hot rolled sheet annealing / pickling process, a cold rolling process, a cold rolled sheet annealing / pickling process, a cold rolling process, a bright annealing process, and a grinding process, the first inclusions do not contain MnO·Al2O3·Cr2O3 whose composition changes, the second inclusions do not contain MgO·Al2O3 whose composition changes, and the total number of inclusions having a maximum equivalent circle diameter of 5 μm or more is 0.5 pieces / mm 2 the following.

[0059] Thus, according to the present embodiment, in order to control the composition of inclusions generated during reduction in the refining process, the slag composition during refining and the concentration of deoxidizing elements and O in the molten steel are adjusted to achieve an appropriate inclusion composition. Thus, it is possible to provide an austenitic stainless steel having excellent surface properties that can reduce the number of inclusions in the surface layer and reduce the variation in piercing and fatigue properties during manufacturing.

[0060] Example

[0061] (Example 1)

[0062] Hereinafter, the present example and comparative examples will be described.

[0063] Austenitic stainless steel scraps and alloy raw materials of each composition of the steel types No. 1 to 55 shown in Table 1 were melted in an electric furnace and then decarburized and refined in an AOD refining step or a converter and vacuum degassing (VOD) refining step.

[0064] [Table 1]

[0065]

[0066] The contents of the elements shown in Table 1 are values ​​expressed in mass %. Sample No. 38 contained 0.001 mass % of REM, Sample No. 39 contained 0.002 mass % of B, and Sample No. 40 contained 0.4 mass % of Nb.

[0067] In addition, limestone, fluorite, and ferrosilicon are added to reduce, deoxidize, and desulfurize the oxidized Cr. At this time, the basicity CaO / SiO2 of the slag is changed within 1.0 to 2.0, and the concentrations of Si and Al used as deoxidizers are changed. It should be noted that after the refined slag is added, bottom blowing of Ar gas is carried out using VOD or LF, and the molten steel is stirred and maintained for 20 minutes with a stirring power of 100W / ton.

[0068] Furthermore, the composition is adjusted in a ladle (after tapping the ladle in the case of AOD refining) and the temperature is adjusted by Ar (argon) bubbling, and a slab is manufactured through a continuous casting process.

[0069] A sample was cut out at 10 mm from the surface of the slab and measured using a SEM (scanning electron microscope) and an EDS (energy dispersive X-ray analyzer). 2 The average inclusion composition of inclusions with an equivalent circle diameter of 5 μm or more existing in the area.

[0070] Furthermore, the steel slabs were subjected to hot rolling (reduction of area of ​​90% or more), hot rolled sheet annealing / pickling, cold rolling, and cold rolled sheet annealing / pickling to produce 0.3 mm cold rolled steel strips.

[0071] Then, the product was cold rolled into a 0.05 mm foil strip, and bright annealed at 1150°C for solution treatment and the like. The surface of the foil product was ground and polished with emery paper, and the thickness at 300 mm was measured. 2 The number of inclusions with a maximum equivalent circle diameter of 5 μm or more in the area.

[0072] [Table 2]

[0073]

[0074] Sample No. 1 to No. 40 in each table corresponds to the present embodiment. Regarding these samples, the steel composition and the slag composition in the refining process meet the range of the above-mentioned embodiment, so the specified hard inclusions (MnO·Al2O3·Cr2O3 and MgO·Al2O3) are few and the number density is low (0.42 pieces / mm 2 Below), good quality can be obtained.

[0075] In contrast, Sample Nos. 41 to 55 in each table correspond to comparative examples. For these samples, the components in the steel and / or the slag components in the refining process are out of the range of the above-mentioned embodiment (underlined in the table), so the prescribed hard inclusions (MnO·Al2O3·Cr2O3 and MgO·Al2O3) are numerous and the number density is high (underlined in the table).

[0076] (Example 2)

[0077] For Sample Nos. 56 to 64 shown in Table 3, sample collection and evaluation were performed in the same manner as in Example 1 except that the bottom blowing gas amount was changed by VOD or LF and the stirring power and stirring holding time were changed as shown in Table 4.

[0078] [Table 3]

[0079]

[0080] [Table 4]

[0081]

[0082] Samples No. 56 to 60 in Table 4 correspond to the present embodiment. Since these samples satisfy the conditions of the present invention confirmed in Example 1, as well as the stirring power and stirring holding time, the specified hard inclusions (MnO·Al2O3·Cr2O3 and MgO·Al2O3) are few and the number density is low, and good quality can be obtained.

[0083] On the other hand, Sample Nos. 61 to 64 in Table 4 correspond to comparative examples. These samples satisfy the conditions of the present invention confirmed in Example 1, but since the stirring power and stirring holding time (underline in the table) are out of the range, the prescribed hard inclusions (MnO·Al2O3·Cr2O3 and MgO·Al2O3) are numerous and the number density is high (underline in the table).

[0084] Therefore, it was confirmed that stainless steel having excellent surface properties can be produced by satisfying the conditions of the present invention as shown in the above-mentioned examples.

Claims

1. A stainless steel for metal foil, characterized in that: It contains C: 0.0001 mass % or more and 0.15 mass % or less, Si: 0.30 mass % or more and 2.0 mass % or less, Mn: 0.1 mass % or more and 15 mass % or less, P: 0.040 mass % or less, Ni: 5 mass % or more and 30 mass % or less, S: 0.0001 mass % or more and 0.01 mass % or less, Cr: 16 mass % or more and 25 mass % or less, Mo: 5 mass % or less, Al: 0.005 mass % or less, Ca: 0.0030 mass % or less, Mg: 0.0010 mass % or less, O: 0.0010 mass % or more and 0.0060 mass % or less, N: 0.0001 mass % or more and 0.5 mass % or less, and the remainder is Fe and inevitable impurities, In the thickness of 0.010 mm or more and 0.2 mm or less, the number of inclusions with a maximum equivalent circle diameter of 5 μm or more is 0.5 / mm 2 the following.

2. The stainless steel for metal foil according to claim 1, characterized in that: The stainless steel for metal foil does not include first inclusions with an average composition of MnO: 10 mass% or more, Cr2O3+Al2O3: 30 mass% or more, and CaO: 10 mass% or less and an equivalent circle diameter of 5 μm or more, and second inclusions with an average composition of MgO: 10 mass% or more, and Al2O3: 20 mass% or more and an equivalent circle diameter of 5 μm or more.

3. The stainless steel for metal foil according to claim 1 or 2, characterized in that: The stainless steel for metal foil further contains at least any one of Cu: 0.1 mass % to 4.0 mass %, REM: 0.00001 mass % to 0.0030 mass %, B: 0.0001 mass % to 0.0050 mass %, Ti: 0.01 mass % to 0.50 mass %, Nb: 0.01 mass % to 0.50 mass %, V: 0.01 mass % to 1.00 mass %, W: 0.01 mass % to 1.00 mass %, Co: 0.01 mass % to 1.00 mass %, and Sn: 0.01 mass % to 1.00 mass %.

4. A stainless steel foil, characterized in that: The thickness is 0.010 mm or more and 0.2 mm or less, the composition contains C: 0.0001 mass % or more and 0.15 mass %, Si: 0.30 mass % or more and 2.0 mass % or less, Mn: 0.1 mass % or more and 15 mass % or less, P: 0.040 mass % or less, Ni: 5 mass % or more and 30 mass % or less, S: 0.0001 mass % or more and 0.01 mass %, Cr: 16 mass % or more and 25 mass %, Mo: 5 mass % or less, Al: 0.005 mass % or less, Ca: 0.0030 mass % or less, Mg: 0.0010 mass % or less, O: 0.0010 mass % or more and 0.0060 mass % or less, N: 0.0001 mass % or more and 0.5 mass %, the remainder is composed of Fe and unavoidable impurities, and the number of inclusions with a maximum equivalent circle diameter of 5 μm or more is 0.5 pieces / mm 2 the following.

5. The stainless steel foil according to claim 4, characterized in that The stainless steel foil further contains at least any one of Cu: 0.1 mass % to 4.0 mass %, REM: 0.00001 mass % to 0.0030 mass %, B: 0.0001 mass % to 0.0050 mass %, Ti: 0.01 mass % to 0.50 mass %, Nb: 0.01 mass % to 0.50 mass %, V: 0.01 mass % to 1.00 mass %, W: 0.01 mass % to 1.00 mass %, Co: 0.01 mass % to 1.00 mass %, and Sn: 0.01 mass % to 1.00 mass %.

6. A method for producing stainless steel for metal foil, comprising producing the stainless steel for metal foil according to any one of claims 1 to 3, characterized in that: Equipped with a refining process using VOD or AOD, In the refining process, Al and Al2O3 contained in the raw material or the ladle are adjusted, deoxidation is carried out using a Fe-Si alloy or metallic Si, and CaO or SiO2 is added, thereby making the slag composition, in terms of mass %, CaO / SiO2: greater than or equal to 1.1 and less than or equal to 1.7, Al2O3: less than or equal to 4.0 mass %, and MgO: less than or equal to 10.0 mass %. Furthermore, after adding the refined slag raw material and the alloy raw material, the molten steel is stirred for more than 5 minutes at a stirring power of more than 50 W / ton.

7. A method for producing a stainless steel foil, comprising producing the stainless steel foil according to claim 4 or 5, characterized in that: Equipped with a refining process using VOD or AOD, In the refining process, Al and Al2O3 contained in the raw material or the ladle are adjusted, deoxidation is carried out using a Fe-Si alloy or metallic Si, and CaO or SiO2 is added, thereby making the slag composition, in terms of mass %, CaO / SiO2: greater than or equal to 1.1 and less than or equal to 1.7, Al2O3: less than or equal to 4.0 mass %, and MgO: less than or equal to 10.0 mass %. Furthermore, after adding the refined slag raw material and the alloy raw material, the molten steel is stirred for more than 5 minutes at a stirring power of more than 50 W / ton.