A preparation method and product of composite aerogel for reducing phenols and carbonyl substances in flue gas
A composite aerogel is developed by modifying cellulose and incorporating copper MOF materials to selectively adsorb phenolic and carbonyl substances in cigarette smoke, addressing the non-selectivity of existing adsorbents and preserving cigarette taste.
Patent Information
- Application Number
- CN202211570821.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-08
AI Technical Summary
Existing adsorbents used in cigarette filters are not selective enough in reducing phenolic and carbonyl substances, often adsorbing tar along with these harmful components, which affects the taste of cigarettes.
A composite aerogel is prepared by modifying cellulose with succinic anhydride and N-ethylcarbamate to graft amino and carboxyl groups, sulfonating the cellulose for hydrophilicity, and incorporating copper MOF materials to form a composite material that selectively adsorbs phenolic and carbonyl substances.
The composite aerogel effectively reduces phenolic and carbonyl substances in cigarette smoke without significantly adsorbing tar, maintaining the taste of cigarettes.
Smart Images

Figure CN115920859B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of aerogel materials, and in particular to a preparation method of a composite aerogel for reducing phenolic and carbonyl substances in flue gas and a product thereof. Background Art
[0002] Smoking is very harmful to the respiratory, gastrointestinal, cardiovascular, nervous system, liver and other organs of the human body. Long-term smoking may cause many diseases such as lung cancer. With the public's active response to the tobacco control campaign, the product development and promotion of low-hazard cigarettes have attracted more and more attention. The various components in cigarette smoke mainly come from the thermal decomposition, thermal synthesis, distillation, polymerization, condensation and other reactions during the combustion of tobacco. As researchers have a deeper understanding of the composition of smoke, technical research on reducing specific harmful components such as phenols and carbonyls has also emerged.
[0003] As far as the existing technology is concerned, the most commonly used method is to use adsorbents to reduce specific harmful components in smoke. For example, in the publication number CN103462221A "A cigarette filter containing an adsorption filter layer and its use", TiO 2 Hydrate nanotubes, TiO 2 Nanopowder, activated carbon fiber and SiO 2 Aerogel cigarette filters use a combination of multiple porous adsorbents to remove harmful components in smoke, but they are not very targeted, so during the adsorption process, they not only adsorb specific harmful components, but also adsorb some tar. The reduction in the amount of tar will greatly affect the taste of cigarettes. Therefore, it is necessary to develop adsorbents that reduce phenolic and carbonyl harmful components without reducing the amount of tar. Summary of the invention
[0004] In order to improve the selectivity of the adsorbent for phenolic and carbonyl harmful components, the present application provides a method for preparing a composite aerogel for reducing phenolic and carbonyl substances in flue gas and a product thereof.
[0005] In the first aspect, the present application provides a method for preparing a composite aerogel for reducing phenols and carbonyl substances in flue gas, which adopts the following technical scheme:
[0006] A method for preparing a composite aerogel for reducing phenolic and carbonyl substances in flue gas comprises the following steps:
[0007] S1: Modification of cellulose: cellulose is preliminarily modified with succinic anhydride and N-ethylcarbamate to obtain preliminarily modified cellulose; the preliminarily modified cellulose is then sulfonated to obtain modified cellulose;
[0008] S2: Preparation of MOF materials: dissolving copper salt in an aqueous solution to obtain a copper salt solution; dissolving mesitylene trimethylolate in a mixed solution of ethanol and DMF to obtain a mesitylene trimethylolate solution; mixing the two solutions and reacting them, filtering, washing and drying them after the reaction is completed to obtain a MOF material;
[0009] S3: Preparation of composite aerogel: The MOF material in step S2 is dispersed in an aqueous solution, and the modified cellulose is dispersed in a mixed solution of n-butanol and water. Under stirring conditions, the MOF material solution is poured into the modified cellulose solution, and after adding ammonia water, the stirring reaction is continued. After the reaction is completed, the reaction solution is stored in a refrigerator, and then the reaction solution is freeze-dried to obtain a composite aerogel.
[0010] By adopting the above technical scheme, in the present application, cellulose is first modified by using succinic anhydride and N-ethylcarbamate to graft amino and carboxyl groups on the surface of the cellulose, the amino groups have a relatively good affinity for carbonyl compounds, and the carboxyl groups have a good affinity for phenolic substances, thereby achieving the adsorption of carbonyl and phenolic substances; and sulfonation treatment is performed on the surface of the cellulose to increase the hydrophilicity of the cellulose, reduce its adsorption of tar, and avoid the change in taste caused by the reduction in the amount of tar.
[0011] Copper MOF material is also introduced into the composite gel in the present application. By utilizing the special hydrogen bonding effect between copper ammonia solution and cellulose, ammonia water is added to the copper MOF material and modified cellulose solution, and the copper MOF material is embedded into the structure of modified cellulose to form a composite material. The copper MOF material is introduced mainly because the copper MOF material can chelate with some carbonyl and phenolic compounds, thereby further reducing the content of carbonyl and phenolic compounds in the flue gas.
[0012] Preferably, in step S1, the specific steps of the preliminary modification treatment are: dispersing cellulose in a mixed solution of ethanol and water, heating, adding sulfuric acid solution, adjusting the pH of the solution to 5-6, then adding succinic anhydride and N-ethylcarbamate thereto, stirring and refluxing reaction, and after the reaction is completed, ultrafiltration, washing and drying are performed to obtain preliminary modified cellulose.
[0013] By adopting the above technical scheme, the present application utilizes the -OH groups on the surface of cellulose, which can undergo a ring-opening reaction with succinic anhydride under acidic conditions and then form ester bonds, thereby grafting carboxylic acid bonds onto the surface of cellulose; similarly, the -OH groups can undergo a substitution reaction with N-ethylcarbamate, thereby grafting amino groups onto the surface of cellulose.
[0014] Preferably, the volume ratio of ethanol to water is (40-60):(40-60); the concentration of cellulose in the mixed solution is 0.1-0.3 g / mL, and the heating temperature is 70-90°C; the mass ratio of cellulose, succinic anhydride and N-ethylcarbamate is 1:(0.05-0.15):(0.06-0.08), and the stirring reflux reaction time is 8-16 hours.
[0015] By adopting the above technical solution, in the present application, by controlling the reaction ratio and reaction conditions, the surface of cellulose can be grafted with active groups as much as possible, thereby increasing the selectivity of the composite gel to the components in the smoke.
[0016] Preferably, the specific steps of the sulfonation are: dispersing the preliminarily modified cellulose in a chloroform solution, then heating it, then dropping chlorosulfonic acid therein, continuing the reaction after the dropping is complete, and after the reaction is complete, ultrafiltration, washing and drying are performed to obtain the modified cellulose.
[0017] By adopting the above technical solution, the cellulose modification process in this application is as follows Figure 1 As shown, further modification with sulfonic acid groups is mainly to enhance its hydrophilicity and reduce its adsorption of tar, thereby reducing the content of phenolic and carbonyl substances without changing the taste of cigarettes.
[0018] Preferably, the concentration of the initially modified cellulose in chloroform is 0.1-0.5 g / mL, the mass ratio of the initially modified cellulose to chlorosulfonic acid is 1:(0.1-0.3), the heating temperature is 40-60° C., and the reaction time is 4-6 h.
[0019] By adopting the above technical solution and controlling the process parameters during the sulfonation process, more groups can be grafted onto the surface of cellulose, thereby better improving the selectivity and adsorption of cellulose.
[0020] Preferably, in step S2, the copper salt is one of copper nitrate, copper chloride and copper sulfate, and its concentration in the aqueous solution is 0.1-0.3 g / mL; the concentration of mesitylene acid in the mixed solution is 0.02-0.04 g / mL; the mass ratio of the copper salt to mesitylene acid is (1-3):(0.5-1.5); the mixing ratio of ethanol to DMF is (15-25):(10-20); the reaction temperature is 80-90°C, and the reaction time is 18-30 h.
[0021] By adopting the above technical solution, the preparation of MOF materials in this application mainly utilizes Cu 2+The oxygen atom in -COOH in mesitylene acid will form an O-Cu-O active site, thus forming a metal cluster during the reaction. The metal cluster can serve as a metal node in the MOF topological structure. On the other hand, Cu 2+ It will also coordinate with the large π bond of the benzene ring of mesitylene acid due to electrostatic interaction, so during the reaction between the two, a porous MOF material with a framework structure will be formed along with the copper ions. In this application, by controlling the reaction conditions, a Cu MOF material with a relatively stable structure can be formed.
[0022] Preferably, in step S2, the specific steps of filtering, washing and drying are as follows: after filtering the reaction solution, washing it with ethanol and DMF for 1 to 2 times, then soaking and washing it with dichloromethane for 1 to 2 times a day for 3 days, and after washing, placing it at 160 to 180° C. for vacuum drying for 10 to 15 hours to obtain MOF material.
[0023] By adopting the above technical solution, the above washing method is adopted in this application mainly to remove unreacted products, and high-temperature drying is adopted mainly to harden the material and form a stable frame structure to avoid its structure from collapsing easily.
[0024] Preferably, in step S3, the concentration of MOF in water is 0.06-0.09 g / mL; the concentration of modified cellulose in the mixed solution is 0.2-0.4 g / mL, the volume ratio of n-butanol to water is (60-80):(20-40); the mass ratio of MOF to modified cellulose is (1-3):(7-9); ammonia water is added to adjust the pH to 8-9, and the stirring reaction time is 3-5 h; after the reaction is completed, it is frozen in a refrigerator below -15°C overnight, and then vacuum freeze-dried for 40-60 h.
[0025] By adopting the above technical solution, in the present application, by controlling the reaction conditions and parameters, the MOF structure can be better introduced into the cellulose gel, thereby better reducing the carbonyl and phenolic substances in the flue gas.
[0026] In the second aspect, a composite aerogel is prepared according to the above-mentioned preparation method.
[0027] In summary, the present application includes at least one of the following beneficial technical effects:
[0028] 1. In this application, cellulose is modified multiple times, and -COOH, -NH and -HSO are attached to its surface. 3The -COOH group can generate strong hydrogen bond adsorption force with the hydroxyl group of phenol, thereby improving its ability to adsorb phenolic substances in smoke; the -NH group has a strong binding force with carbonyl compounds, thus further reducing the content of carbonyl compounds in smoke; and the -HSO 3 The group has strong hydrophilicity and can reduce the adsorption of tar by the gel.
[0029] 2. The MOF structure of Cu is also introduced into the aerogel of the present application. First, it has a pore structure, and copper ions have a complexing effect on phenols and carbonyl substances. Therefore, the combination of the two can selectively reduce the content of phenols and carbonyl compounds. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic diagram of cellulose modification in this application.
[0031] Figure 2 Schematic diagram of the filling of composite aerogel during the testing process of the present application. DETAILED DESCRIPTION
[0032] Example 1
[0033] S1: Modification of cellulose: Schematic diagram of the modification steps can be seen Figure 1 , the specific preparation method is as follows:
[0034] 10 g of cellulose was dispersed in 50 mL of a mixed solution of ethanol and water in a volume ratio of 50:50, heated to 80°C, a dilute sulfuric acid solution was added, and the pH of the solution was adjusted to 5-6. Then, 1 g of succinic anhydride and 0.7 g of N-ethylcarbamate were added thereto, and the mixture was stirred and refluxed for 12 h. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain preliminary modified cellulose.
[0035] 11.1 g of the preliminary modified cellulose was dispersed in 40 mL of chloroform, then heated to 50°C, and 2.22 g of chlorosulfonic acid was added dropwise thereto. After the addition was completed, the reaction was continued for 5 hours. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain the modified cellulose.
[0036] S2: MOF material preparation:
[0037] 2.2 g of copper nitrate was dissolved in 10 mL of aqueous solution to obtain a copper nitrate solution; 1.2 g of mesitylene trimethylolate was dissolved in a mixed solution of 20 mL of ethanol and 15 mL of DMF to obtain a mesitylene trimethylolate melt; the two solutions were mixed, heated to 85°C, and reacted for 24 hours. After the reaction was completed, the reaction solution was filtered and washed twice with a mixed solution of 50:50 ethanol and DMF; then it was placed in a dichloromethane solution for immersion, and the dichloromethane was replaced every day until it was immersed for 3 days, and then filtered, and the filter residue was placed in a vacuum drying oven at 170°C for vacuum drying for 12 hours to obtain a MOF material.
[0038] S3: Preparation of composite aerogels
[0039] 2.0 g of MOF material in step S2 was dispersed in 28 mL of aqueous solution, 8 g of modified cellulose was dispersed in a mixed solution of 19 mL of n-butanol and 8 mL of water, and the MOF material solution was poured into the modified cellulose solution under stirring. After adding ammonia water, the pH of the solution was adjusted to 8-9, and the stirring was continued for 4 h. After the reaction was completed, the reaction solution was stored in a refrigerator at -20 °C overnight, and then the reaction solution was vacuum freeze-dried for 48 h to obtain a composite aerogel, and its average pore size was measured to be 12.4 nm and the specific surface area was 307.66 m 2 / g.
[0040] Comparative Example 1
[0041] The same as Example 1, except that the cellulose was not modified, that is, there was no step S1, and MOF reacted directly with cellulose to obtain a composite aerogel; the average pore size was measured to be 16.8 nm, and the specific surface area was 286.55 m 2 / g.
[0042] Comparative Example 2
[0043] The method is basically the same as Example 1, except that the modification steps are different and no N-ethylcarbamate is added. The details are as follows:
[0044] 10 g of cellulose was dispersed in 50 mL of a mixed solution of ethanol and water in a volume ratio of 50:50, heated to 80°C, a dilute sulfuric acid solution was added, and the pH of the solution was adjusted to 5-6. Then 1 g of succinic anhydride was added thereto, and the mixture was stirred and refluxed for 12 hours. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain preliminary modified cellulose.
[0045] The prepared composite aerogel has an average pore size of 15.4 nm and a specific surface area of 297.53 m 2 / g.
[0046] Comparative Example 3
[0047] The method is basically the same as Example 1, except that the modification steps are different and succinic anhydride is not added, as follows:
[0048] 10 g of cellulose was dispersed in 50 mL of a mixed solution of ethanol and water in a volume ratio of 50:50, heated to 80°C, a dilute sulfuric acid solution was added, and the pH of the solution was adjusted to 5-6. Then 0.7 g of N-ethylcarbamate was added thereto, and the mixture was stirred and refluxed for 12 hours. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain preliminary modified cellulose.
[0049] The prepared composite aerogel has an average pore size of 15.6 nm and a specific surface area of 294.64 m 2 / g.
[0050] Comparative Example 4
[0051] It is basically the same as Example 1, except that the primary modified cellulose is used to composite with the MOF material.
[0052] The prepared composite aerogel has an average pore size of 15.8 nm and a specific surface area of 292.52 m 2 / g.
[0053] Comparative Example 5
[0054] The method is basically the same as Example 1, except that the modified cellulose is directly used to prepare the aerogel.
[0055] The average pore size of the prepared aerogel is 21.4 nm and the specific surface area is 231.72 m 2 / g.
[0056] Filtration effect test: Buy a cigarette filter (plastic transparent filter), remove the original filler, and then fill it with 50mg of the above aerogel. Take a commercially available Baisha cigarette (12mg tar, 1.2mg nicotine, 13mg carbon monoxide), cut off the original filter cotton part of the cigarette, and stick it on the filter filled with aerogel (assembly diagram as shown in the figure). Figure 2 A filter tip not filled with aerogel was used as a control.
[0057] A simulated smoking machine was used to collect smoke produced by cigarettes, and the tar content was tested by gas chromatography; the formaldehyde, acetaldehyde, acrolein, crotonaldehyde, acetone, and 2-butanone contents were tested by high performance liquid chromatography; and the phenol, hydroquinone, catechol, and resorcinol contents were tested by liquid chromatography.
[0058] Table 1
[0059] Unprocessed Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Tar(mg) 10.8 9.4 8.2 9.3 9.5 8.6 9.3 Formaldehyde(ug) 46.4 29.7 40.5 40.1 28.4 30.2 34.6 Acetaldehyde(ug) 550.4 434.7 479.7 471.3 430.5 442.1 449.7 Acrolein (ug) 45.9 34.7 41.2 39.8 33.6 36.2 38.4 Crotonaldehyde(ug) 50.1 39.1 44.3 44.5 38.4 41.2 44.6 Acetone(ug) 101.3 73.6 86.9 85.2 72.4 75.6 78.9 2-Butanone(ug) 70.3 60.3 68.2 67.8 59.4 62.4 65.7 Phenol(ug) 5.4 3.8 4.6 3.7 4.5 4.1 4.3 Hydroquinone (ug) 12.5 8.6 10.9 8.2 10.9 8.9 10.2 Catechol(ug) 16.4 11.7 13.7 11.1 13.8 12.2 12.9 Resorcinol(ug) 2.7 ND 2.5 ND 2.1 ND 1.4
[0060] Note: ND in the table means not detected.
[0061] It can be seen from the data in Table 1 that both Example 1 and the comparative example have certain adsorption properties and can remove some harmful substances in the flue gas. Compared with the control product without adding aerogel, the components in the flue gas are reduced to a certain extent.
[0062] Compared with Comparative Example 1, the cellulose in Example 1 is not modified. From the data, the adsorption of tar in Comparative Example 1 is relatively high, but the adsorption of tar in Example 1 is relatively low, which may be because the grafting of sulfonic acid groups increases its hydrophilicity, thereby reducing the adsorption of tar. The adsorption of carbonyl substances and phenolic substances in Example 1 is significantly better than that in Comparative Example 1, which may be because the modification and grafting of -COOH and -NH increases the adsorption of the two substances.
[0063] Compared with Example 1 and Comparative Example 2, there is no grafted -NH group in Comparative Example 2. Although the adsorption of phenolic substances in Comparative Example 2 is slightly better than that in Example 1, its adsorption of carbonyl substances is significantly lower than that in Example 1. This may be because there is no grafted -NH group in Comparative Example 2, so its grafted -COOH groups are slightly more, so its adsorption performance for phenols is slightly improved, but it has no -NH group, and its adsorption of carbonyl substances is significantly reduced.
[0064] Compared with Example 3, Example 1 does not have a grafted -COOH group in Example 3. Although the adsorption of carbonyl substances in the comparative example is slightly better than that in Example 1, its adsorption of phenolic substances is significantly lower than that in Example 1. This may be because there is no grafted -COOH group in Comparative Example 3, so its grafted -NH groups are slightly more, so its adsorption performance for carbonyl substances is slightly improved, but it has no -COOH group, and its adsorption of phenolic substances is significantly reduced.
[0065] Compared with Example 1, there is no grafted sulfonic acid group in Comparative Example 4. From the data, the adsorption of tar in Comparative Example 4 is increased and the adsorption of other substances is decreased compared with Example 1. This may be because more tar is adsorbed, which reduces the adsorption of carbonyl and phenolic substances.
[0066] Compared with Example 5, Example 1 does not introduce MOF into Example 5; its adsorption to carbonyl and phenolic substances is reduced, which may be because there is no complexation effect of MOF material, and its adsorption to the two types of substances is reduced.
[0067] Example 2
[0068] S1: Modification of cellulose:
[0069] 10 g of cellulose was dispersed in 80 mL of a mixed solution of ethanol and water in a volume ratio of 60:40, heated to 90°C, a dilute sulfuric acid solution was added, and the pH of the solution was adjusted to 5-6. Then, 0.5 g of succinic anhydride and 0.8 g of N-ethylcarbamate were added thereto, and the mixture was stirred and refluxed for 16 hours. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain preliminary modified cellulose.
[0070] 9.6 g of the preliminary modified cellulose was dispersed in 25 mL of chloroform, then heated to 60°C, and 1.15 g of chlorosulfonic acid was added dropwise thereto. After the addition was completed, the reaction was continued for 4 hours. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain the modified cellulose.
[0071] S2: MOF material preparation:
[0072] 1.5 g of copper chloride was dissolved in 12 mL of aqueous solution to obtain a copper nitrate solution; 0.8 g of mesitylene trimethylolate was dissolved in a mixed solution of 20 mL of ethanol and 20 mL of DMF to obtain a mesitylene trimethylolate melt; the two solutions were mixed, heated to 90°C, and reacted for 18 hours. After the reaction was completed, the reaction solution was filtered and washed twice with a mixed solution of 50:50 ethanol and DMF; then it was placed in a dichloromethane solution for immersion, and the dichloromethane was replaced every day until it was immersed for 3 days, and then filtered. The filter residue was placed in a vacuum drying oven at 180°C for vacuum drying for 10 hours to obtain a MOF material.
[0073] S3: Preparation of composite aerogels
[0074] 1.5 g of MOF material in step S2 was dispersed in 25 mL of aqueous solution, 8.5 g of modified cellulose was dispersed in a mixed solution of 17 mL of n-butanol and 4 mL of water, and the MOF material solution was poured into the modified cellulose solution under stirring. After adding ammonia water, the pH of the solution was adjusted to 8-9, and the stirring was continued for 3 h. After the reaction was completed, the reaction solution was stored in a refrigerator at -20 ° C overnight, and then the reaction solution was vacuum freeze-dried for 60 h to obtain a composite aerogel; the average pore size was measured to be 12.9 nm, and the specific surface area was 305.4 m 2 / g
[0075] Example 3
[0076] S1: Modification of cellulose:
[0077] 10 g of cellulose was dispersed in 45 mL of a mixed solution of ethanol and water in a volume ratio of 40:60, heated to 70°C, a dilute sulfuric acid solution was added, and the pH of the solution was adjusted to 5-6. Then, 1.5 g of succinic anhydride and 0.6 g of N-ethylcarbamate were added thereto, and the mixture was stirred and refluxed for 16 hours. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain preliminary modified cellulose.
[0078] 9.8 g of the preliminary modified cellulose was dispersed in 60 mL of chloroform, then heated to 40°C, and 2.5 g of chlorosulfonic acid was added dropwise thereto. After the addition was completed, the reaction was continued for 6 hours. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain the modified cellulose.
[0079] S2: MOF material preparation:
[0080] 3.0 g of copper sulfate was dissolved in 10 mL of aqueous solution to obtain a copper nitrate solution; 1.5 g of mesitylene acid was dissolved in a mixed solution of 17 mL of ethanol and 20 mL of DMF to obtain a mesitylene acid melt; the two solutions were mixed, heated to 80°C, and reacted for 30 hours. After the reaction was completed, the reaction solution was filtered and washed twice with a mixed solution of 50:50 ethanol and DMF; then it was placed in a dichloromethane solution for immersion, and the dichloromethane was replaced every day until it was immersed for 3 days, and then filtered. The filter residue was placed in a vacuum drying oven at 160°C for vacuum drying for 15 hours to obtain a MOF material.
[0081] S3: Preparation of composite aerogels
[0082] 2.0 g of MOF material in step S2 was dispersed in 8 mL of aqueous solution, 8 g of modified cellulose was dispersed in a mixed solution of 16 mL of n-butanol and 4 mL of water, and the MOF material solution was poured into the modified cellulose solution under stirring. After adding ammonia water, the pH of the solution was adjusted to 8-9, and the stirring was continued for 5 h. After the reaction was completed, the reaction solution was stored in a refrigerator at -20 ° C overnight, and then the reaction solution was vacuum freeze-dried for 40 h to obtain a composite aerogel; the average pore size was measured to be 12.2 nm, and the specific surface area was 308.97 m 2 / g.
[0083] Example 4
[0084] S1: Modification of cellulose:
[0085] 10 g of cellulose was dispersed in 55 mL of a mixed solution of ethanol and water in a volume ratio of 50:50, heated to 80°C, a dilute sulfuric acid solution was added, and the pH of the solution was adjusted to 5-6. Then, 1.5 g of succinic anhydride and 0.8 g of N-ethylcarbamate were added thereto, and the mixture was stirred and refluxed for 16 hours. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain preliminary modified cellulose.
[0086] 10 g of the preliminary modified cellulose was dispersed in 40 mL of chloroform, then heated to 50°C, 3.0 g of chlorosulfonic acid was added dropwise thereto, and after the addition was completed, the reaction was continued for 6 hours. After the reaction was completed, ultrafiltration, washing and drying were performed to obtain the modified cellulose.
[0087] S2: MOF material preparation:
[0088] 2.5 g of copper chloride was dissolved in 10 mL of aqueous solution to obtain a copper nitrate solution; 1.3 g of mesitylene acid was dissolved in a mixed solution of 17 mL of ethanol and 20 mL of DMF to obtain a mesitylene acid molten solution; the two solutions were mixed, heated to 80°C, and reacted for 30 hours. After the reaction was completed, the reaction solution was filtered and washed twice with a mixed solution of 50:50 ethanol and DMF; then it was placed in a dichloromethane solution for immersion, and the dichloromethane was replaced every day until it was immersed for 3 days, and then filtered, and the filter residue was placed in a vacuum drying oven at 170°C for vacuum drying for 13 hours to obtain a MOF material.
[0089] S3: Preparation of composite aerogels
[0090] 1.0 g of MOF material in step S2 was dispersed in 12 mL of aqueous solution, 9 g of modified cellulose was dispersed in a mixed solution of 18 mL of n-butanol and 6 mL of water, and the MOF material solution was poured into the modified cellulose solution under stirring. After adding ammonia water, the pH of the solution was adjusted to 8-9, and the stirring was continued for 5 h. After the reaction was completed, the reaction solution was stored in a refrigerator at -20 °C overnight, and then the reaction solution was vacuum freeze-dried for 48 h to obtain a composite aerogel, and its average pore size was measured to be 13.4 nm and the specific surface area was 302.77 m 2 / g.
[0091] The performance of removing smoke components from the composite aerogels prepared in Examples 2 to 4 was tested, and the results are shown in Table 2.
[0092] Table 2
[0093] Unprocessed Example 2 Example 3 Example 4 Tar(mg) 10.8 9.2 9.6 9.7 Formaldehyde(ug) 46.4 33.5 27.4 27.5 Acetaldehyde(ug) 550.4 445.7 422.6 429.3 Acrolein (ug) 45.9 36.2 32.4 32.4 Crotonaldehyde(ug) 50.1 42.3 36.7 37.4 Acetone(ug) 101.3 76.4 71.5 72.5 2-Butanone(ug) 70.3 63.5 58.4 57.4 Phenol(ug) 5.4 3.4 4.0 3.5 Hydroquinone (ug) 12.5 8.4 8.9 8.4 Catechol(ug) 16.4 10.8 12.0 10.8 Resorcinol(ug) 2.7 ND ND ND
[0094] From the data in Table 2, it can be seen that with the change of process parameters, the performance of the prepared aerogel will fluctuate to a certain extent, but it maintains good adsorption performance for carbonyl and phenolic compounds.
[0095] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a composite aerogel for reducing phenols and carbonyl substances in flue gas, comprising the following steps: S1: Modification of cellulose: cellulose is preliminarily modified with succinic anhydride and N-ethylcarbamate to obtain preliminarily modified cellulose; the preliminarily modified cellulose is then sulfonated to obtain modified cellulose; S2: Preparation of MOF material: dissolving copper salt in aqueous solution to obtain copper salt solution; dissolving trimesic acid in a mixed solution of ethanol and DMF to obtain trimesic acid solution; mixing the two solutions and reacting them, filtering, washing and drying them after the reaction is completed to obtain MOF material; S3: Preparation of composite aerogel: The MOF material in step S2 is dispersed in an aqueous solution, and the modified cellulose is dispersed in a mixed solution of n-butanol and water. Under stirring conditions, the MOF material solution is poured into the modified cellulose solution, and after adding ammonia water, the stirring reaction is continued. After the reaction is completed, the reaction solution is stored in a refrigerator, and then the reaction solution is freeze-dried to obtain a composite aerogel; In step S1, the specific steps of the preliminary modification treatment are: dispersing cellulose in a mixed solution of ethanol and water, heating, adding sulfuric acid solution, adjusting the pH of the solution to 5-6, then adding succinic anhydride and N-ethylcarbamate thereto, stirring and refluxing, and after the reaction is completed, ultrafiltration, washing and drying to obtain preliminary modified cellulose; The volume ratio of ethanol to water is (40-60):(40-60); the concentration of cellulose in the mixed solution is 0.1-0.3 g / mL, and the heating temperature is 70-90° C.; the mass ratio of cellulose, succinic anhydride and N-ethylcarbamate is 1:(0.05-0.15):(0.06-0.08), and the stirring reflux reaction time is 8-16 hours; The specific steps of the sulfonation are: dispersing the preliminarily modified cellulose in a chloroform solution, then heating it, then dropping chlorosulfonic acid therein, and after the dropping is completed, continuing the reaction, and after the reaction is completed, ultrafiltration, washing and drying are performed to obtain the modified cellulose; The concentration of the initially modified cellulose in chloroform is 0.1-0.5 g / mL, the mass ratio of the initially modified cellulose to chlorosulfonic acid is 1:(0.1-0.3), the heating temperature is 40-60° C., and the reaction time is 4-6 hours.
2. The method for preparing a composite aerogel for reducing phenolic and carbonyl substances in flue gas according to claim 1, characterized in that: In the step S2, the copper salt is one of copper nitrate, copper chloride and copper sulfate, and its concentration in the aqueous solution is 0.1-0.3 g / mL; the concentration of trimesic acid in the mixed solution is 0.02-0.04 g / mL; the mass ratio of the copper salt to trimesic acid is (1-3):(0.5-1.5); the mixing ratio of ethanol to DMF is (15-25):(10-20); the reaction temperature is 80-90°C, and the reaction time is 18-30 hours.
3. The method for preparing a composite aerogel for reducing phenolic and carbonyl substances in flue gas according to claim 1, characterized in that: In step S2, the specific steps of filtering, washing and drying are as follows: after filtering the reaction solution, washing it with ethanol and DMF for 1 to 2 times, then soaking and washing it with dichloromethane for 1 to 2 times a day for 3 days, and after washing, placing it at 160 to 180° C. for vacuum drying for 10 to 15 hours to obtain MOF material.
4. The method for preparing a composite aerogel for reducing phenolic and carbonyl substances in flue gas according to claim 1, characterized in that: In the step S3, the concentration of MOF in water is 0.06-0.09 g / mL; the concentration of modified cellulose in the mixed solution is 0.2-0.4 g / mL, the volume ratio of n-butanol to water is (60-80):(20-40); the mass ratio of MOF to modified cellulose is (1-3):(7-9); ammonia water is added to adjust the pH to 8-9, and the stirring reaction time is 3-5 hours; after the reaction is completed, it is frozen in a refrigerator below -15°C overnight, and then vacuum freeze-dried for 40-60 hours.
5. The composite aerogel is prepared according to the preparation method according to any one of claims 1 to 4.