A blue protective film and preparation method thereof
Through the use of EVA-PE-EVA composite membrane structure and inorganic fillers, the problems of poor protection effect and high cost of existing protective clothing materials are solved, and efficient and durable protective effects and low-cost production are achieved.
Patent Information
- Application Number
- CN202211383288.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-07
AI Technical Summary
Existing disposable protective clothing materials, such as PP and PE, have problems such as large fiber gaps, poor protection effect, or high cost and the addition of other substances to reduce the protection effect, resulting in easy passage of harmful substances and bacterial viruses, and strength and durability. insufficient.
EVA-PE-EVA composite membrane structure is used to prepare EVA composite through materials such as vinyl acetate, initiators, methyl methacrylate, ethylene monomers, polyethylene glycol, polylactic acid and paraffin. Combined with the PE film layer, increase protection The film has strength, flexibility and moisture permeability, and enhances tensile properties and bonding fastness through inorganic fillers.
The protective film is effectively prevented from penetration of harmful substances and bacteria, improves the protective effect and strength, and at the same time reduces the amount of PE, reduces production costs, and improves the heat resistance and softness of the protective film.
Smart Images

Figure BDA0003929480620000061 
Figure BDA0003929480620000081 
Figure BDA0003929480620000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of protective films, and more specifically, to a blue protective film and a preparation method thereof. Background Art
[0002] Reusable protective products that have been used for a long time, such as white coats and cotton gloves, are gradually being abandoned as people's understanding of medical protection technology improves. The reason is that if the repeatedly used protective clothing is not thoroughly disinfected or contaminated with bacteria during the transfer process, it may cause secondary infection of medical staff and patients. People began to use disposable protective equipment, which will be directly destroyed in a centralized manner after use, greatly reducing the occurrence and spread of diseases and improving people's health level. Therefore, disposable protective equipment has become the first choice for medical protective equipment.
[0003] At present, the materials commonly used for disposable protective clothing are mainly PP, PE, SMS, etc. Among them, PP has a lower cost and is the first choice for most manufacturers to produce disposable protective products. However, PP is extruded and spun, and then randomly arranged into a mesh curtain by airflow or machinery, and then fixed by hot rolling. Although this non-woven fabric has a low cost, as a protective clothing, its fiber gap is large, and harmful substances or bacteria and viruses can easily pass through the fabric and contact the human body, which can easily cause infection; PE has a good protective effect when used to prepare protective clothing, but PE is relatively expensive. Usually manufacturers will add other substances to mix and use to reduce costs, which will lead to a reduction in protective effect; SMS spunbond and melt-blown composite products have the advantages of high strength, good filtration performance, no adhesive, and non-toxicity, but its fibers are arranged in a certain direction, so it is easy to split from the right angle direction and has poor strength. Summary of the invention
[0004] In order to provide protective equipment with good protective effect, good strength and low production cost, the present application provides a blue protective film and a preparation method thereof.
[0005] In the first aspect, the present application provides a blue protective film, which adopts the following technical solution:
[0006] A blue protective film, the blue protective film comprises a first EVA film layer, a PE film layer and a second EVA film layer in sequence, wherein the first VAE film layer and the second EVA film layer are both made of raw materials including the following parts by weight:
[0007] EVA compound 80-90 parts
[0008] 2-5 parts of lubricant
[0009] Metallocene polyethylene 0-15 parts;
[0010] The EVA composite is prepared by the following method:
[0011] A: First, mix the vinyl acetate monomer and the initiator and add them into the reactor for polymerization. Heat the system temperature to 230-270°C and the polymerization pressure to 2500-2600 kg / cm 2 , adding methyl methacrylate, and then introducing ethylene monomer into the system for reaction to obtain EVA polymer;
[0012] B: melt-granulating the EVA polymer prepared in step A with polyethylene glycol, polylactic acid and paraffin to obtain a masterbatch;
[0013] C: The masterbatch prepared in step B is melt-granulated with PE to obtain an EVA composite.
[0014] By adopting the above technical solution, the gap of the prepared protective film is small, and harmful substances or bacteria and viruses are not easy to penetrate the protective film. In addition, in the present application, the protective effect and strength of the blue protective film are further improved by using the EVA-PE-EVA composite film, which can effectively prevent harmful substances and bacteria from passing through the protective film to contact the human body and is not easy to be damaged. Furthermore, in the present application, by using the composite film, the amount of PE is reduced while ensuring the protective effect, thereby reducing the production cost of the enterprise.
[0015] EVA is a soft and elastic material. It can be used to prepare a protective film to increase the softness and elasticity of the protective film and prevent it from cracking. However, its hot melt phase is poor and its surface strength is low. When used to prepare a protective film, it is easy for the surface of the protective film to be damaged. In this regard, the present application first polymerizes vinyl acetate, an initiator, methyl methacrylate and ethylene monomers at a specific temperature and pressure to obtain an EVA polymer. The EVA polymer prepared by this method can improve the surface strength and heat resistance of the EVA film, making the EVA film less likely to be damaged.
[0016] Among them, the lubricant increases the smoothness of the EVA film surface, reduces the adhesion during the preparation process, and increases the metallocene polyethylene, which can increase the tensile strength of the EVA composite film and make it less likely to break.
[0017] The EVA copolymer prepared in this application does not absorb water, has a hard texture, and has poor moisture permeability. When used to prepare a protective film, the protective film has poor moisture permeability and poor softness. In this regard, polyethylene glycol is added in this application to improve the moisture permeability of the protective film, and at the same time, it is used in conjunction with polylactic acid to enhance the softness of the protective film, which is beneficial to the use of the protective film. Among them, polylactic acid can increase the bonding strength between the EVA film layer and the PE film layer, and paraffin can increase the fluidity of the system, so that polyethylene glycol, polylactic acid and EVA polymer can be mixed evenly. At the same time, PE is added in this application to prepare an EVA composite in order to stably connect the EVA film layer and the PE film layer in the composite film formation through the action of PE.
[0018] Preferably, the initiator is an azo initiator or a peroxide initiator.
[0019] Preferably, the lubricant is stearamide, erucamide or oleamide.
[0020] Preferably, the materials used in the process of preparing the EVA composite are as follows in parts by weight:
[0021] 40-50 parts of vinyl acetate monomer
[0022] 1-2 parts of initiator
[0023] 40-60 parts of ethylene monomer
[0024] Methyl methacrylate 10-15 parts
[0025] 10-20 parts of polyethylene glycol
[0026] Polylactic acid 10-15 parts
[0027] 1-2 parts paraffin
[0028] PE1~5 parts.
[0029] By adopting the above technical solution, the ratio of raw materials for preparing EVA composites is optimized, the protective effect, softness, moisture permeability and strength of the protective film prepared using the EVA composite are further improved, and the applicability of the protective film is improved.
[0030] Preferably, the average molecular weight of the EVA polymer is 1600-3000.
[0031] By optimizing the molecular weight of the EVA polymer, the elasticity and softness of the EVA compound are further improved, and the elasticity and softness of the protective film are improved. Preferably, the average molecular weight of the polyethylene glycol is 1500-4000.
[0032] By optimizing the average molecular weight of polyethylene glycol, the moisture permeability of the protective film is further improved, and the softness of the protection is also further improved.
[0033] Preferably, the first EVA film layer and the second EVA film layer also include 10 to 15 parts by weight of inorganic filler, and each part of the inorganic filler is composed of nano-silicon dioxide, talcum powder and calcium carbonate in a weight ratio of (10 to 15):1:(10 to 20).
[0034] The air permeability of the membrane layer prepared by the EVA composite is poor. In this regard, the addition of inorganic fillers in the present application can enhance the air permeability of the membrane prepared by the EVA composite, wherein the nano-silicon dioxide increases the tensile strength of the membrane, so that the membrane has good tensile properties. When stretched, interfacial peeling occurs between the polymer and the calcium carbonate particles, and interconnected winding pores or channels are formed around the calcium carbonate particles. These pores and channels give the EVA membrane layer a moisture permeability function, and talcum powder improves the fluidity of calcium carbonate and nano-silicon dioxide.
[0035] Preferably, the PE film layer is prepared by mixing a PE and EVA composite in a weight ratio of (10-12):5.
[0036] By adopting the above-mentioned preparation method, the PE film layer is firmly bonded to the first EVA film layer and the second EVA film layer, and is not easy to be delaminated during the use of the overlayer. PE and EVA are two different substances. They are not easy to bond in the process of preparing the composite film, and the bonding is stable. In this regard, the PE and EVA composite is used in the overlayer of the PE film. According to the principle of similar compatibility, the PE film layer can be stably bonded to the first EVA film layer and the second EVA film layer when composited into a film, and it is not easy to be delaminated. The first EVA film layer, the second EVA film layer and the PE film layer all contain EVA composites. The compatibility between the EVA composites is better than that between PE and EVA, and it is easier to connect. And when the EVA composite is added to the PE film layer, while ensuring the protective effect of the protective film, the amount of PE is reduced and the cost is reduced.
[0037] Preferably, the molecular weight of the PE is 50,000-100,000.
[0038] The PE film layer prepared by using the PE prepared with the above specific molecular weight has good softness and good adhesion with the EVA film layer.
[0039] Preferably, the first EVA film layer and the second EVA film layer further include 5 to 10 parts by weight of polycaprolactone, and the average molecular weight of the polycaprolactone is 60,000 to 120,000.
[0040] The addition of inorganic fillers in this application will reduce the elasticity of the protective film, and the protective film will not easily return to its original shape after being pulled by external forces. In this regard, polycaprolactone is added in this application. By adding polycaprolactone, the elasticity of the protective film is increased, and the possibility of deformation due to external impact is reduced. In addition, polycaprolactone has good compatibility with EVA composites and metallocene polyethylene, which is conducive to the subsequent preparation of the film.
[0041] In a second aspect, the present application provides a method for preparing a blue protective film, using the following technical solution:
[0042] A method for preparing a blue protective film comprises the following preparation steps:
[0043] S1, mixing an EVA compound, a lubricant and a metallocene polyethylene to prepare a mixture A;
[0044] S2, mixing PE and EVA compounds to obtain mixture B
[0045] S3. Add the mixture A obtained in step S1, the mixture A obtained in step S1, and the mixture A obtained in step S1 into the lower extruder, the middle extruder, and the upper extruder of the three-layer co-extruder respectively, and compound and biaxially stretch them through the co-extrusion die to obtain a blue protective film which is, from bottom to top, a first EVA film layer, a PE film layer, and a second EVA film layer.
[0046] The blue protective film prepared by the above method has good protective effect, light stretch, softness, air permeability and moisture permeability. The present application adopts a three-layer extrusion method to prepare the protective film, so that the protective film can be stably connected and not easy to delaminate.
[0047] Preferably, the temperature of the heating zone 1 of the upper extruder and the lower extruder is 150-160°C, the temperature of the heating zone 2 is 180-190°C, the temperature of the heating zone 3 is 200-210°C, the temperature of the heating zone 4 is 200-220°C, the temperature of the heating zone 5 is 170-180°C, and the temperature of the heating zone 6 is 150-160°C;
[0048] The temperature of heating zone 1 of the middle layer extruder is 170-180°C, the temperature of heating zone 2 is 190-200°C, the temperature of heating zone 3 is 200-210°C, the temperature of heating zone 4 is 200-210°C, the temperature of heating zone 5 is 180-190°C, and the temperature of heating zone 6 is 160-170°C.
[0049] By adopting the above technical scheme, the prepared protective film has good physical properties, and by reasonably setting the heating temperatures of the upper extruder, the middle extruder and the lower extruder, it has good gloss, flatness, softness, moisture permeability and protective effect.
[0050] In summary, this application has the following beneficial effects:
[0051] 1. The present application provides a blue protective film, which includes a first EVA film layer, a PE film layer and a second EVA film layer in sequence. The structure of the composite film makes it difficult for harmful substances or bacteria and viruses to penetrate the protective film, while reducing the amount of PE used and reducing the production cost of the enterprise. Among them, the first VAE film layer and the second EVA film layer are both prepared from EVA composites, lubricants and metallocene polyethylene, and the EVA composite is prepared from vinyl acetate monomer, initiator, methyl methacrylate, ethylene monomer, polyethylene glycol, polylactic acid, paraffin and PE. The EVA composite prepared by the present application is used to prepare an EVA film with a lubricant and metallocene polyethylene, which can improve the ability of the EVA film to protect against harmful substances and viruses, and can also improve the elongation at break, tensile strength and heat resistance of the EVA film.
[0052] 2. The present application improves the moisture permeability of the EVA film by adding inorganic fillers prepared from nano-silicon dioxide, talcum powder and calcium carbonate, wherein the nano-silicon dioxide increases the tensile strength of the film, so that the film has good tensile properties. When stretched, interfacial peeling occurs between the polymer and the calcium carbonate particles, and interconnected winding pores or channels are formed around the calcium carbonate particles. These pores and channels give the EVA film layer a moisture permeability function, and the talcum powder improves the fluidity of calcium carbonate and nano-silicon dioxide.
[0053] 3. In the present application, the PE film layer is prepared by mixing PE and EVA composites. By mixing PE and EVA composites, the PE film layer can be stably bonded with the first EVA film layer and the second EVA film layer when composited into a film, and is not easy to delaminate. According to the principle of similar compatibility, the first EVA film layer, the second EVA film layer and the PE film layer all contain EVA composites. The compatibility between EVA composites is better than that between PE and EVA, and they are easier to connect. DETAILED DESCRIPTION
[0054] Preparation Example
[0055] Preparation Example 1
[0056] An EVA composite is prepared by the following method:
[0057] A: According to weight parts, 40 parts of vinyl acetate monomer and 1 part of initiator were mixed and added to the reactor for polymerization. The system temperature was heated to 230°C and the polymerization pressure was 2500 kg / cm 2 , add 10 parts of methyl methacrylate, and then introduce 40 parts of ethylene monomer into the system for reaction to obtain EVA polymer;
[0058] B: melt-granulate the EVA polymer prepared in step A with 10 parts of polyethylene glycol, 10 parts of polylactic acid and 1 part of paraffin wax in parts by weight to obtain a masterbatch;
[0059] C: The masterbatch prepared in step B is melt-granulated with 1 part of PE to obtain an EVA composite.
[0060] Wherein, the initiator is cyclohexanone peroxide
[0061] Paraffin wax has 30 carbon atoms.
[0062] The lubricant is stearamide.
[0063] The molecular weight of polyethylene glycol is 5000.
[0064] Polylactic acid was purchased from Ningbo Shunxin Import & Export Co., Ltd. under the brand name ingeo and the grade number 3D870.
[0065] The average molecular weight of PE is 40,000.
[0066] The molecular weight of EVA polymer is 1500.
[0067] The difference between Preparation Examples 2 to 3 and Preparation Example 1 is that the raw material dosage and test parameters for preparing some EVA composites are consistent with those in Preparation Example 1, as shown in Table 1:
[0068] Table 1 Raw material dosage and test parameters of EVA composite
[0069]
[0070] Preparation Example 4
[0071] An EVA composite, the difference between this preparation example and preparation example 1 is that the heating temperature in step A is 250°C and the polymerization pressure is 2600kg / cm 2 The remaining raw material types, amounts and experimental steps are consistent with those in Preparation Example 1.
[0072] The molecular weight of EVA polymer is 1600.
[0073] Preparation Example 5
[0074] An EVA composite, the difference between this preparation example and preparation example 1 is that the heating temperature in step A is 270°C and the polymerization pressure is 2500kg / cm 2 The remaining raw material types, amounts and experimental steps are consistent with those in Preparation Example 1.
[0075] The molecular weight of EVA polymer is 3000.
[0076] Preparation Example 6
[0077] An EVA composite, the difference between this preparation example and preparation example 1 is that the average molecular weight of the polyethylene glycol added in step B is 1500, and the other raw material types, amounts and experimental steps are consistent with those in preparation example 1.
[0078] Preparation Example 7
[0079] An EVA composite, the difference between this preparation example and preparation example 1 is that the average molecular weight of the polyethylene glycol added in step B is 4000, and the other raw material types, amounts and experimental steps are consistent with those in preparation example 1.
[0080] Example
[0081] Example 1
[0082] A blue protective film is prepared by the following method:
[0083] S1. Mix 80 parts of the EVA compound from Preparation Example 1 and 2 parts of a lubricant, by weight, to prepare a mixture A;
[0084] S2, 30 parts by weight of PE are used to prepare mixture B;
[0085] S3. Add the mixture A obtained in step S1, the mixture B obtained in step S2, and the mixture A obtained in step S1 into the lower extruder, the middle extruder, and the upper extruder of the three-layer co-extruder respectively, compound and biaxially stretch through the co-extrusion die head to obtain a blue protective film which comprises a first EVA film layer, a PE film layer, and a second EVA film layer from bottom to top.
[0086] Among them, the temperature of the heating zone 1 of the upper extruder and the lower extruder is 150°C, the temperature of the heating zone 2 is 180°C, the temperature of the heating zone 3 is 200°C, the temperature of the heating zone 4 is 200°C, the temperature of the heating zone 5 is 170°C, and the temperature of the heating zone 6 is 150°C;
[0087] The temperature of heating zone 1 of the middle layer extruder is 170°C, the temperature of heating zone 2 is 190°C, the temperature of heating zone 3 is 200°C, the temperature of heating zone 4 is 200°C, the temperature of heating zone 5 is 180°C, and the temperature of heating zone 6 is 160°C.
[0088] The lubricant is erucamide.
[0089] Metallocene polyethylene was purchased from Shanghai Yi Zeng Plasticizing Co., Ltd. under the brand name of Priman, and the melt mass flow rate was 3.8 g / 10 min.
[0090] The average molecular weight of PE is 40,000.
[0091] Example 2
[0092] A blue protective film, which is different from Example 1 in that: the raw materials of the first VAE film layer and the second EVA film layer are further added with 5 parts by weight of metallocene polyethylene, and the amounts, types and test steps of the remaining raw materials are consistent with those in Example 1.
[0093] The difference between Examples 3 and 4 and Example 2 is that the amounts of raw materials used in the first VAE film layer and the second EVA film layer are different, and the remaining experimental steps are consistent with Example 2.
[0094] The materials and types of raw materials in Examples 1 to 4 are shown in Table 1:
[0095] Table 1 Materials and types of raw materials in Examples 1 to 4
[0096]
[0097]
[0098] Example 5
[0099] A blue protective film. The difference between this embodiment and embodiment 2 is that the EVA compound comes from preparation example 4, and the types, amounts and experimental steps of other raw materials are consistent with those of embodiment 2.
[0100] Example 6
[0101] A blue protective film. The difference between this embodiment and embodiment 2 is that the EVA compound comes from preparation example 5, and the types, amounts and experimental steps of other raw materials are consistent with those of embodiment 2.
[0102] Example 7
[0103] A blue protective film. The difference between this embodiment and embodiment 2 is that the EVA compound comes from preparation example 6, and the types, amounts and experimental steps of other raw materials are consistent with those of embodiment 2.
[0104] Example 8
[0105] A blue protective film. The difference between this embodiment and embodiment 2 is that the EVA compound comes from preparation example 7, and the types, amounts and experimental steps of other raw materials are consistent with those of embodiment 2.
[0106] Example 9
[0107] A blue protective film, the difference between this embodiment and embodiment 2 is that: the first EVA film layer and the second EVA film layer also include 10 parts by weight of inorganic filler, and each part of the inorganic filler is composed of nano silicon dioxide, talcum powder and calcium carbonate in a weight ratio of 10:1:10.
[0108] Example 10
[0109] A blue protective film, the difference between this embodiment and embodiment 2 is that: the first EVA film layer and the second EVA film layer also include 15 parts by weight of inorganic filler, and each part of the inorganic filler is composed of nano silicon dioxide, talcum powder and calcium carbonate in a weight ratio of 15:1:20.
[0110] Embodiment 11
[0111] A blue protective film, the difference between this embodiment and embodiment 2 is that the PE film layer is prepared by mixing PE and EVA composites in a weight ratio of 10:5, and the remaining raw material types, amounts and experimental steps are consistent with those in embodiment 2.
[0112] The EVA compound is from Preparation Example 1, and the molecular weight of PE is 40,000.
[0113] Example 12
[0114] A blue protective film, the difference between this embodiment and embodiment 2 is that the PE film layer is prepared by mixing PE and EVA composites in a weight ratio of 12:5, and the remaining raw material types, amounts and experimental steps are consistent with those in embodiment 2.
[0115] The EVA compound is from Preparation Example 1, and the molecular weight of PE is 110,000.
[0116] Example 13
[0117] A blue protective film. The difference between this embodiment and embodiment 12 is that the molecular weight of PE is 50,000, and the other raw material types, amounts and experimental steps are consistent with those of embodiment 14.
[0118] Embodiment 14
[0119] A blue protective film. The difference between this embodiment and embodiment 12 is that the molecular weight of PE is 100,000, and the other raw material types, amounts and experimental steps are consistent with those of embodiment 14.
[0120] Embodiment 15
[0121] A blue protective film. The difference between this embodiment and embodiment 10 is that the first EVA film layer and the second EVA film layer also include 5 parts by weight of polycaprolactone, the molecular weight of polycaprolactone is 60000, and the remaining raw material types, amounts and experimental steps are consistent with embodiment 10.
[0122] Example 16
[0123] A blue protective film. The difference between this embodiment and embodiment 10 is that the first EVA film layer and the second EVA film layer also include 10 parts by weight of polycaprolactone, the molecular weight of polycaprolactone is 120000, and the remaining raw material types, amounts and experimental steps are consistent with embodiment 10.
[0124] Comparative Example
[0125] Comparative Example 1
[0126] A blue protective film. The difference between this comparative example and Example 2 is that the EVA polymer is commercially available and purchased from Dongguan Weicai Plastic Raw Materials Co., Ltd., model number 4260. The other raw material types, amounts and experimental steps are consistent with Example 2.
[0127] Performance testing
[0128] The protective film prepared in this application was tested for breaking strength, breaking elongation, moisture permeability, filtration efficiency, bonding strength and hygiene standards.
[0129] Detection method / test method
[0130] For breaking strength, breaking elongation, moisture permeability and filtration efficiency, refer to GB 19082-2009.
[0131] Adhesion strength: The protective films prepared in Examples 1 to 16 were heated at 200°C for 30 seconds, then placed in a mixture of ice and water, cooled, taken out, and observed to see if the surface of the protective film bulged.
[0132] The test data are shown in Table 3:
[0133] Table 3 Performance test data
[0134]
[0135] It can be seen from Examples 1 to 16 and Comparative Example 1 in combination with Table 3 that the EVA film prepared by using the EVA composite prepared in the present application and the lubricant and metallocene polyethylene has good breaking strength, breaking elongation, moisture permeability and filtration efficiency.
[0136] Comparison between Example 2 and Comparative Example 2 shows that the EVA composite prepared by the present application can further improve the breaking strength, breaking elongation, moisture permeability and filtration efficiency of the EVA film.
[0137] Comparison between Example 2 and Examples 9 to 10 shows that the inorganic filler can effectively improve the breaking strength and moisture permeability of the protective film.
[0138] Comparison of Example 2 with Examples 11 to 12 shows that the PE film layer prepared by using the PE and EVA composite has good adhesion to the EVA film layer.
[0139] Comparison of Example 10 with Examples 15 to 16 shows that the addition of polycaprolactone can effectively improve the problem of reduced elongation at break of the protective film caused by inorganic fillers.
[0140] The sanitation standard refers to GB15979-2002. The test data is shown in Table 4:
[0141] Table 4 Performance test experimental data
[0142]
[0143] It can be seen from Examples 1 to 16 and Comparative Example 1 in combination with Table 3 that the hygienic standards of the EVA film prepared by using the EVA composite and lubricant prepared by the present application and metallocene polyethylene are higher than the national standards.
[0144] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A blue protective film, characterized in that: The blue protective film comprises a first EVA film layer, a PE film layer and a second EVA film layer in sequence, wherein the first EVA film layer and the second EVA film layer are both made of raw materials including the following parts by weight: EVA compound 80~90 parts 2~5 parts of lubricant Metallocene polyethylene 0-15 parts; The EVA composite is prepared by the following method: A: First, mix the vinyl acetate monomer and the initiator and add them into the reactor for polymerization. Heat the system temperature to 230-270°C and the polymerization pressure to 2500-2600 kg / cm 2 , adding methyl methacrylate, and then introducing ethylene monomer into the system for reaction to obtain EVA polymer; B: melt-granulating the EVA polymer prepared in step A with polyethylene glycol, polylactic acid and paraffin to obtain a masterbatch; C: melt-granulating the masterbatch prepared in step B with PE to obtain an EVA composite; The materials used in the preparation of the EVA composite are as follows in parts by weight: 40~50 parts of vinyl acetate monomer 1~2 parts of initiator 40~60 parts of ethylene monomer Methyl methacrylate 10~15 parts 10~20 parts of polyethylene glycol Polylactic acid 10~15 parts 1~2 parts paraffin PE 1~5 parts; The PE film layer is prepared by mixing PE and EVA composites in a weight ratio of (10-12):5; The method comprises the following preparation steps: S1, mixing an EVA compound, a lubricant and a metallocene polyethylene to prepare a mixture A; S2, mixing PE and EVA compounds to obtain a mixture B; S3. Add the mixture A obtained in step S1, the mixture B obtained in step S2, and the mixture A obtained in step S1 into the lower extruder, the middle extruder, and the upper extruder of the three-layer co-extruder in a mass ratio of (2-3):0.5:(2-3), respectively, and compound and biaxially stretch through the co-extrusion die to obtain a blue protective film comprising a first EVA film layer, a PE film layer, and a second EVA film layer from bottom to top.
2. A blue protective film according to claim 1, characterized in that: The average molecular weight of the EVA polymer is 1600-3000.
3. A blue protective film according to claim 1, characterized in that: The average molecular weight of the polyethylene glycol is 1500-4000.
4. A blue protective film according to claim 1, characterized in that: The first EVA film layer and the second EVA film layer also include 10 to 15 parts by weight of inorganic filler, and each part of the inorganic filler is composed of nano-silicon dioxide, talcum powder and calcium carbonate in a weight ratio of (10 to 15): 1: (10 to 20).
5. The blue protective film according to claim 1, characterized in that: The molecular weight of the PE is 50,000-100,000.
6. The blue protective film according to claim 1, characterized in that: The first EVA film layer and the second EVA film layer also include 5 to 10 parts by weight of polycaprolactone, and the average molecular weight of the polycaprolactone is 60,000 to 120,000.
7. The blue protective film according to claim 1, characterized in that: The temperature of the heating zone 1 of the upper extruder and the lower extruder is 150~160℃, the temperature of the heating zone 2 is 180~190℃, the temperature of the heating zone 3 is 200~210℃, the temperature of the heating zone 4 is 200~220℃, the temperature of the heating zone 5 is 170~180℃, and the temperature of the heating zone 6 is 150~160℃; The temperature of heating zone 1 of the middle layer extruder is 170~180℃, the temperature of heating zone 2 is 190~200℃, the temperature of heating zone 3 is 200~210℃, the temperature of heating zone 4 is 200~210℃, the temperature of heating zone 5 is 180~190℃, and the temperature of heating zone 6 is 160~170℃.