A method for purifying ammonium rhenate

By controlling the dissolution and crystallization process of ammonium perrylate using a disc turbine stirrer, large agglomerates are broken up, and particle size and morphology are adjusted. This solves the problem of uneven purity and particle size of ammonium perrylate in traditional methods, and produces high-purity ammonium perrylate crystals with regular morphology, which are suitable for modern metallurgical fields.

CN115924979BActive Publication Date: 2024-11-26JINCHUAN GROUP CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211421884.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-14
Publication Date
2024-11-26
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

Traditional methods for purifying ammonium perrye crystallization cannot achieve controllable particle size and morphology, resulting in low purity and uneven particle size distribution of ammonium perrye, which cannot meet the high powder performance requirements of modern metallurgy. Furthermore, existing methods use large amounts of inorganic acids and ammonia, making waste liquid treatment difficult.

Method used

Ammonium perrylate was gradually heated and dissolved under normal pressure using a disc turbine stirrer. The stirring intensity and cooling rate were controlled. Large agglomerates were broken up by high-speed mechanical stirring, and crystallization was carried out within a specific temperature range. The precipitation rate and particle size of ammonium perrylate were controlled. Finally, high-purity ammonium perrylate crystals were obtained by vacuum filtration and natural air drying.

Benefits of technology

This method achieves ammonium perrylate crystals with regular morphology, controllable particle size, uniform particle size distribution, purity higher than 99.99%, and large specific surface area, meeting the high powder performance requirements of modern metallurgy and reducing the difficulty of waste liquid treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115924979B_ABST
    Figure CN115924979B_ABST
Patent Text Reader

Abstract

The invention discloses a method for purifying ammonium rhenate, comprising the following steps: using low-purity crude ammonium rhenate as a raw material, adding distilled water, stirring and heating to dissolve, and filtering to obtain a supersaturated ammonium rhenate solution; passing the supersaturated ammonium rhenate solution into a cooling crystallization reactor, and using a disc turbine stirrer for high-speed mechanical stirring, controlling the stirring intensity and the cooling rate, cooling to ‑10~0 ℃, maintaining in this temperature range, and continuing high-speed mechanical stirring to obtain a solid-liquid mixture; filtering the obtained solid-liquid mixture, and naturally air-drying, that is, obtaining a particle-refined high-purity ammonium rhenate crystal. The present invention can effectively realize the controllability of the particle size of the ammonium rhenate crystal, optimize the morphology of the ammonium rhenate crystal, improve the purity of the ammonium rhenate, the uniformity of the particle size distribution and the specific surface area, and has a good prospect for engineering application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare metal element recovery, and in particular to a method for purifying ammonium rhenate. Background Art

[0002] Ammonium rhenate is an important raw material for preparing rhenium metal powder. The prepared rhenium powder can not only be processed into rhenium ingots and rhenium bars, but also is an important raw material for alloy series such as tungsten-rhenium alloy, aerospace materials, and high-temperature resistant mechanical equipment parts. In addition, the high-purity rhenium powder prepared by hydrogen reduction of ammonium rhenate has excellent powder properties and is also used in the preparation of rhenium materials in the aerospace field. It is a key high-quality rhenium resource.

[0003] In view of the rapid development of metallurgical technology, the traditional crystallization purification method cannot meet the requirements of modern metallurgical technology for the performance of ammonium rhenate powder, especially in the modern metallurgical field as a raw material for preparing high-purity rhenium powder and powder injection molding and powder jet molding. Therefore, improving the purity of ammonium rhenate and achieving controllability of its particle size and morphology have an important impact on the application effect of ammonium rhenate in the field of modern metallurgy. At present, the crystallization and purification technology of ammonium rhenate cannot achieve the controllability of its particle size and morphology. The macroscopic morphology and particle size distribution of the purified ammonium rhenate are uneven, and the purity is not high, which cannot meet the high powder performance requirements of ammonium rhenate in the field of modern metallurgy.

[0004] Patent CN201910939501.9 discloses a method for purifying crude ammonium rhenate from copper smelting, which uses pure water-nitric acid-ammonia water to purify ammonium rhenate. The existing patent uses a large amount of inorganic acid and ammonia water in the process of purifying ammonium rhenate, and the waste liquid generated in the process is difficult to treat. Summary of the invention

[0005] In view of the shortcomings of the above-mentioned prior art, the present invention provides a method for purifying ammonium rhenate.

[0006] The present invention is achieved through the following technical solutions.

[0007] A method for purifying ammonium rhenate comprises the following steps:

[0008] (1) Using low-purity crude ammonium rhenate as a raw material, gradually adding distilled water under normal pressure, stirring and heating until the crude ammonium rhenate is dissolved, and filtering to obtain a supersaturated ammonium rhenate solution with a temperature of 120 to 130° C.;

[0009] (2) Cooling crystallization of supersaturated ammonium rhenate solution: The supersaturated ammonium rhenate solution is introduced into a cooling crystallization reactor and stirred mechanically with a disc turbine stirrer at a high speed, with the stirring intensity controlled at 500 to 900 rpm and the cooling rate controlled at 2 to 4°C / min, and cooled to -10 to 0°C, and maintained at this temperature, and continued to be stirred mechanically with a disc turbine stirrer at a high speed, wherein the stirring intensity is 500 to 900 rpm and the stirring time is 8 to 10 hours, to obtain a solid-liquid mixture;

[0010] (3) The solid-liquid mixture obtained in step (2) is filtered and naturally air-dried to obtain finely divided high-purity ammonium rhenate crystals.

[0011] Furthermore, in the step (1), the purity of the crude ammonium rhenate is 93-95 wt%.

[0012] Furthermore, in the step (1), the crude ammonium rhenate is heated at a heating rate of 2°C to 3°C / min until it is dissolved.

[0013] Furthermore, in the step (2), the temperature is lowered at a rate of 2 to 4°C / min. When the system temperature drops to 0°C, the crystallization is maintained at this temperature for 1 to 2 hours, and then the temperature of the cooling crystallization reactor is adjusted to -10 to 0°C, and high-speed stirring is continued.

[0014] The ammonium rhenate crystals prepared by the method of the invention have regular morphology, controllable particle size, uniform particle size distribution, large specific surface area and a purity higher than 99.99%.

[0015] The design mechanism of the present invention is:

[0016] The present invention utilizes the property that ammonium rhenate is slightly soluble in cold water, controls the dissolution rate of ammonium rhenate in water by adjusting the heating rate, and removes insoluble solid impurities by suction filtration to obtain a hot supersaturated solution of ammonium rhenate; in the crystallization and purification process, utilizes the strong shear force of a disc turbine stirrer to break large particle agglomerates under high-speed stirring, and the broken small particles grow into ammonium rhenate crystals through secondary crystallization, and controls the mechanical stirring intensity and cooling rate to obtain high-purity ammonium rhenate crystals with uniform particle size distribution after condensation and crystallization. The advantages of this method are that large particle crystals can be broken by a disc turbine stirrer, the precipitation rate of crystals can be controlled by changing the cooling rate to achieve purification, and the particle size of ammonium rhenate can be controlled by changing the stirring intensity to obtain ammonium rhenate powder with uniform particle size distribution, regular crystal morphology, and large specific surface area.

[0017] The beneficial effects of the present invention are as follows:

[0018] 1. The present invention adopts a disc turbine stirrer to break large particle agglomerates under high-speed stirring, and the broken small particles grow into ammonium rhenate crystals through secondary crystallization; the mechanical stirring intensity and the cooling rate are regulated to achieve controllable precipitation rate and particle size of ammonium rhenate crystals, thereby improving the purity, particle uniformity and specific surface area of ​​ammonium rhenate.

[0019] 2. The present invention crystallizes and purifies low-purity crude ammonium rhenate in an aqueous solution by regulating the cooling rate, mechanical stirring intensity and crystallization time in different temperature ranges, thereby obtaining high-purity ammonium rhenate crystals with regular macroscopic morphology, uniform particle size distribution, large specific surface area and controllable particle size. Within the stirring speed range of 500 to 900 rpm, the median diameter of ammonium rhenate is inversely proportional to the stirring intensity, and the crystal morphology changes from irregular agglomerated particles to square crystals of similar size.

[0020] 3. The present invention can effectively realize the controllability of the particle size of ammonium rhenate crystals, optimize the morphology of ammonium rhenate crystals, improve the purity of ammonium rhenate, the uniformity of particle size distribution and the specific surface area, and has good engineering application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a scanning electron microscope image of ammonium rhenate in Example 1.

[0022] Figure 2 This is the particle size distribution diagram of ammonium rhenate in Example 1.

[0023] Figure 3 This is a scanning electron microscope image of ammonium rhenate in Example 2.

[0024] Figure 4 This is the particle size distribution diagram of ammonium rhenate in Example 2.

[0025] Figure 5 This is a scanning electron microscope image of ammonium rhenate in Example 2.

[0026] Figure 6 This is the particle size distribution diagram of ammonium rhenate in Example 2.

[0027] Figure 7 This is a scanning electron microscope image of ammonium rhenate in Comparative Example 1.

[0028] Figure 8 This is the particle size distribution diagram of ammonium rhenate in Comparative Example 1. DETAILED DESCRIPTION

[0029] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0030] A method for purifying ammonium rhenate comprises the following steps:

[0031] (1) using crude ammonium rhenate with a purity of 93-95 wt% as a raw material, gradually adding distilled water under normal pressure, and stirring and heating at a heating rate of 2°C-3°C / min until the crude ammonium rhenate is dissolved, and filtering to obtain a supersaturated ammonium rhenate solution with a temperature of 120-130°C;

[0032] (2) Cooling crystallization of supersaturated ammonium rhenate solution: The supersaturated ammonium rhenate solution is passed into a cooling crystallization reactor for crystallization purification, and a disc turbine stirrer is used for high-speed mechanical stirring, and the stirring intensity is controlled to be 500-900 rpm and the cooling rate is 2-4°C / min. When the system temperature drops to 0°C, the crystallization is maintained at this temperature for 1-2 hours, and then the temperature of the cooling crystallization reactor is adjusted to -10-0°C, and maintained in this temperature range, and a disc turbine stirrer is continued for high-speed mechanical stirring, wherein the stirring intensity is 500-900 rpm and the stirring time is 8-10 hours to obtain a solid-liquid mixture;

[0033] (3) The solid-liquid mixture obtained in step (2) is filtered and naturally air-dried to obtain finely divided high-purity ammonium rhenate crystals.

[0034] In the above step (2), a disc turbine agitator is used to break up large particle agglomerates, so that the large particle agglomerates are broken up, and the broken small particles grow into ammonium rhenate crystals through secondary crystallization. By adjusting the mechanical stirring intensity and the cooling rate, the particle size of ammonium rhenate and the precipitation rate of ammonium rhenate can be controlled, and the impurity compounds with strong water solubility are retained in the mother liquor, thereby optimizing the morphology of the ammonium rhenate crystals, improving the purity of ammonium rhenate, the uniformity of particle size distribution and the specific surface area. When the mechanical stirring intensity is in the range of 500 to 900 rpm, the particle size of the ammonium rhenate decreases with the increase of the stirring intensity, and the crystal morphology changes from irregular agglomerated particles to square crystals with similar morphology.

[0035] The ammonium rhenate crystals prepared by the method of the present invention have regular morphology, controllable particle size, uniform particle size distribution, and a specific surface area greater than 20m 2 / kg, the median particle size is less than 80um, and its purity is higher than 99.99%.

[0036] Example 1

[0037] Weigh 300 g of low-purity crude ammonium rhenate (purity of 93.22 wt%) and place it in a container. Gradually add distilled water to the container, stir thoroughly and heat at a heating rate of 2°C / min to dissolve the raw materials. When a small amount of ammonium rhenate solid remains at the bottom of the container, stop adding distilled water and stop heating, filter at a constant temperature to obtain a clarified ammonium rhenate thermal supersaturated solution at a temperature of 130°C; pass the obtained thermal supersaturated solution into a cooling crystallization reactor, use a disc turbine stirrer to mechanically stir and condense and crystallize, control the stirring intensity and cooling rate, cool to 0°C at a stirring intensity of 900 rpm and a cooling rate of 4°C / min, crystallize for 2 hours under this condition, adjust the temperature of the cooling crystallization reactor to -10°C, maintain this temperature and continue to mechanically stir at 900 rpm for 10 hours, filter the obtained material by suction, and naturally air-dry, thereby obtaining high-purity ammonium rhenate crystal powder with fine particles. After testing, the median diameter of ammonium rhenate is 71.17 μm and the specific surface area is 26.93 m 2 / kg, with a purity of approximately 99.995%.

[0038] Example 2

[0039] Weigh 300 g of low-purity crude ammonium rhenate (purity of 94.72 wt%) and place it in a container. Gradually add distilled water to the container, stir thoroughly and heat at a heating rate of 2°C / min to dissolve the raw materials. When a small amount of ammonium rhenate solid remains at the bottom of the container, stop adding distilled water and stop heating, filter at a constant temperature to obtain a clarified ammonium rhenate thermal supersaturated solution at a temperature of 125°C; pass the obtained thermal supersaturated solution into a cooling crystallization reactor, use a disc turbine stirrer to mechanically stir and condense and crystallize, control the stirring intensity and cooling rate, cool to 0°C at a stirring intensity of 800 rpm and a cooling rate of 3°C / min, crystallize for 1.5 hours under this condition, adjust the reactor temperature to -5°C, maintain this temperature and continue to mechanically stir at 800 rpm for 9 hours, filter the obtained material by suction, and air-dry naturally to obtain high-purity micronized ammonium rhenate crystal powder. After testing, the median diameter of ammonium rhenate is 78.37 μm and the specific surface area is 24.56 m 2 / kg, with a purity of approximately 99.992%.

[0040] Example 3

[0041] 300 g of low-purity crude ammonium rhenate (purity of 93.56 wt%) was weighed and placed in a container, distilled water was gradually added to the container, and the mixture was fully stirred and heated at a heating rate of 3°C / min to dissolve the raw materials. When a small amount of ammonium rhenate solid remained at the bottom of the container, the addition of distilled water and the heating were stopped, and the mixture was filtered at a constant temperature to obtain a clarified thermal supersaturated solution of ammonium rhenate at a temperature of 120°C; the obtained thermal supersaturated solution was passed into a cooling crystallization reactor, and a disc turbine stirrer was used for mechanical stirring to condense and crystallize, and the stirring intensity and the cooling rate were controlled. The stirring intensity was 700 rpm, the cooling rate was 4°C / min, the temperature was cooled to 0°C, and crystallization was carried out under this condition for 1 hour. After adjusting the temperature of the reactor to 0°C, the temperature was maintained at this temperature and mechanical stirring was continued at 700 rpm for 8 hours. The obtained material was filtered and naturally air-dried, thereby obtaining high-purity micronized ammonium rhenate crystal powder. After testing, the median diameter of ammonium rhenate is 79.32μm, the specific surface area is 23.54m2 / kg, and the purity is about 99.990%.

[0042] Comparative Example 1

[0043] Weigh 300g of low-purity crude ammonium rhenate (purity 94.79wt%) and place it in a container. Gradually add distilled water to the container, stir thoroughly and heat at a heating rate of 2°C / min to dissolve the raw materials. When a small amount of ammonium rhenate solid remains at the bottom of the container, stop adding distilled water and stop heating. Filter at a constant temperature to obtain a clear supersaturated ammonium rhenate solution. Pass the supersaturated solution into a cooling crystallization reactor, cool and crystallize without mechanical stirring, the cooling rate is 1°C / min, cool to -10°C, the crystallization time is 12 hours, filter the solid-liquid mixture, and air dry naturally to obtain ammonium rhenate crystal powder. After testing, the median diameter of ammonium rhenate is 218.6μm and the specific surface area is 9.636m 2 / kg, with a purity of approximately 97.87%.

[0044] The scanning electron microscope images of the ammonium rhenate crystals after cooling and crystallization in the above Examples 1-3 and Comparative Example 1 ( Figure 1 , Figure 3 , Figure 5 ) and particle size distribution diagram ( Figure 2 , Figure 4 , Figure 6 ) It can be seen that the present invention can break up large particle agglomerates under high-speed stirring, and the broken small particles grow into ammonium rhenate crystals through secondary crystallization; by adjusting the stirring intensity and the cooling rate, the crystal size is reduced, the uniformity of the particle size distribution is enhanced, the specific surface area is increased, the purity is improved, and the crystal morphology is changed from irregular agglomerated crystals to regular square crystals.

[0045] The particle size of the ammonium rhenate obtained in Examples 1-3 decreases with the increase of stirring intensity, and has a relatively uniform particle size distribution. The obtained powder has a large specific surface area and a high purity. The particle size of the ammonium rhenate obtained in Comparative Example 1 is uneven, the crystal morphology is irregular, and the purity is lower than that of Examples 1-3.

[0046] It can be concluded from the above experimental results that the present invention is used to crystallize and purify crude ammonium rhenate with low purity, and large particle agglomerates are broken under high-speed stirring, and the broken small particles grow into ammonium rhenate crystals through secondary crystallization; the particle size of the ammonium rhenate crystals can be controlled, the morphology of the ammonium rhenate crystals is optimized, and the purity of the ammonium rhenate, the uniformity of the particle size distribution and the specific surface area are improved.

[0047] According to the advantages of the present invention, the particle size of ammonium rhenate crystals can be effectively controlled, the morphology of ammonium rhenate crystals can be optimized, the purity of ammonium rhenate, the uniformity of particle size distribution and the specific surface area can be improved, and the invention has good engineering application prospects.

[0048] The above is only a preferred embodiment of the present invention and does not limit the invention. It should be pointed out that for ordinary technicians in this field, under the technical enlightenment provided by the present invention, other equivalent improvements can be made, all of which can achieve the purpose of the present invention and should be regarded as the protection scope of the present invention.

Claims

1. A method for purifying ammonium rhenate, characterized in that: The method comprises the following steps: (1) Using low-purity crude ammonium rhenate as a raw material, the purity of the crude ammonium rhenate is 93-95 wt %, adding distilled water under normal pressure, stirring and heating until the crude ammonium rhenate is dissolved, and filtering to obtain a supersaturated ammonium rhenate solution with a temperature of 125-130° C.; (2) Cooling crystallization of supersaturated ammonium rhenate solution: The supersaturated ammonium rhenate solution is introduced into a cooling crystallization reactor and stirred mechanically at high speed by a disc turbine stirrer, the stirring intensity is controlled to be 500 to 900 rpm, and the cooling rate is controlled to be 2 to 4°C / min. When the system temperature drops to 0°C, the crystallization is maintained at this temperature for 1 to 2 hours, and then the temperature of the cooling crystallization reactor is adjusted to -10 to 0°C, and maintained at this temperature, and high-speed mechanical stirring is continued by a disc turbine stirrer, wherein the stirring intensity is 500 to 900 rpm and the stirring time is 8 to 10 hours to obtain a solid-liquid mixture; (3) The solid-liquid mixture obtained in step (2) is filtered and naturally air-dried to obtain finely divided high-purity ammonium rhenate crystals.

2. The method for purifying ammonium rhenate according to claim 1, characterized in that: In the step (1), the crude ammonium rhenate is heated at a heating rate of 2°C to 3°C / min until it is dissolved.

Citation Information

Patent Citations

  • Method for purifying crude ammonium rhenate produced through copper smelting

    CN110683585A

  • Method for purifying high purity ammonium rhenate from liquid containing ammonium rhenate

    CN103172122A

  • Ammonium rhenate with uniform granularity and preparation method thereof

    CN110606511A

  • Ammonium rhenate purification system

    CN111333116A

  • Purification process of copper smelting byproduct ammonium perrhenate

    CN111874952A