A kind of ultraviolet resistant aging quartz stone plate and preparation method thereof
By using methyl methacrylate-methyl methacrylate copolymer to blend with quartz sand and powder, combined with silane coupling agent and other materials, to form dense quartz stone sheets, the problem of poor aging resistance in the prior art is solved. , significantly improves hardness and gloss, and improves the overall quality of the board.
Patent Information
- Application Number
- CN202211618244.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-15
Smart Images

Figure BDA0004000856730000031 
Figure BDA0004000856730000041 
Figure BDA0004000856730000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building decoration, and in particular to an ultraviolet resistant aged quartz stone plate and a preparation method thereof. Background Art
[0002] As an important part of building materials, natural stone is widely used in the fields of construction, furniture, etc. due to its diverse colors and easy mining. However, with the excessive increase in its mining volume and low mining utilization rate, the mining of natural stone is restricted and the supply is insufficient to meet market demand. Artificial quartz stone is a new type of man-made building material with high strength, high hardness, high temperature resistance, and corrosion resistance. At present, as a substitute for natural stone, it is widely used in building panels, wall, ground construction and other architectural decoration fields. Artificial quartz stone is mainly composed of quartz stone and resin, and is pressed into large-sized plates by machines and equipment under certain physical and chemical conditions.
[0003] However, the resin raw materials commonly used in artificial quartz stone are thermosetting resins, mainly orthophthalic or isophthalic unsaturated polyester resins. The resin has poor aging resistance, and the boards are very prone to yellowing and darkening. In addition, the boards lack toughness, are brittle, and are prone to cracking. At the same time, the surface hardness and glossiness are insufficient, and improvement requires coating and surface crystallization treatment. The effect of this treatment method is not long-lasting, so the quality of the boards cannot be guaranteed. Summary of the invention
[0004] The invention provides an ultraviolet resistant aging quartz stone plate and a preparation method thereof, so as to simultaneously improve the aging resistance, hardness and glossiness of the quartz stone plate.
[0005] In order to solve the above technical problems, one of the purposes of the present invention is to provide a UV-resistant aged quartz stone plate, comprising the following components in parts by weight:
[0006] Methyl methacrylate-methyl methacrylate copolymer: 9 parts to 18 parts;
[0007] Quartz sand: 35-60 parts;
[0008] Quartz powder: 25-33 parts;
[0009] Silane coupling agent: 0.08-1 part;
[0010] Curing agent: 0.08-0.25 parts;
[0011] Accelerator: 0.008-0.03 parts;
[0012] Color paste: 0.05-0.7 parts;
[0013] Among them, the mesh number of quartz sand is 6 mesh-120 mesh, and the mesh number of quartz powder is 324-400 mesh.
[0014] By adopting the above scheme, the present application adopts methyl methacrylate-methyl methacrylate copolymer and the filler in the system to be blended with each other, and the generated board material is relatively dense, and the hardness of the resin material is high, which can significantly improve the hardness of the final board material, reduce the shedding of particles during the surface polishing process, improve the glossiness of the board surface, and simultaneously improve the aging resistance of the board material.
[0015] As a preferred embodiment, the quartz stone plate further comprises 10-20 parts by weight of solid particles, wherein the solid particles are one or more of silica rock, shell powder, and mica powder.
[0016] As a preferred embodiment, the silane coupling agent is one or more of 3-(trimethoxysilyl)propyl methacrylate, 3-(2;3-epoxypropoxy)propyltrimethoxysilane, and γ-aminopropyltriethoxysilane.
[0017] As a preferred embodiment, the curing agent is tert-butyl permaleate.
[0018] As a preferred embodiment, the mass ratio of the quartz sand, quartz powder and solid particles is (7-8):5:(2-4).
[0019] As a preferred solution, the quartz sand includes 8-16 mesh, 26-40 mesh, and 70-120 mesh quartz sand in a mass ratio of 1:2:2.
[0020] As a preferred embodiment, the accelerator is JHT8-D.
[0021] In order to solve the above technical problems, the second object of the present invention is to provide a method for preparing a UV-resistant aging quartz stone plate, comprising the following steps:
[0022] S1, weighing quartz sand, quartz powder and solid particles and mixing them evenly to obtain an aggregate mixture, weighing methyl methacrylate-methyl methacrylate copolymer, silane coupling agent, curing agent, accelerator and color paste and mixing them evenly to obtain a first mixed slurry;
[0023] S2, pouring the aggregate mixture into a stirring device, adding the first mixed slurry under stirring conditions, stirring evenly, to obtain a second mixed slurry;
[0024] S3, injecting the second mixed slurry into the mold and evenly spreading it, pressing it under vacuum to obtain a embryonic plate, placing the embryonic plate and the mold into a curing furnace for heating and curing treatment, demolding, surface treatment of the embryonic plate, and coating to obtain a finished product.
[0025] As a preferred embodiment, in S2, the aggregate mixture is poured into a mixing device, and the first mixed slurry is added under stirring at 10-20 rpm, and after stirring at 10-20 rpm for 1-3 min, the mixture is stirred at 30-60 rpm for 2-5 min to obtain a second mixed slurry.
[0026] As a preferred solution, in S3, the conditions for pressing under vacuum are: vacuum degree 0.8-1MPa, and the frequency of pressing changes to 25HZ for 5s, 30HZ for 5s, 35HZ for 10s, 45HZ for 20s, 40HZ for 5s, and 35HZ for 5s.
[0027] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:
[0028] The present application adopts methyl methacrylate-methyl methacrylate copolymer to replace the traditional unsaturated polyester resin raw material, and mixes it with quartz powder and quartz sand aggregates of different mesh sizes to form a dense board. The aging resistance is excellent, the resin has a strong adhesion to the aggregate, and the particles are not easy to fall off during the surface treatment process. The resin has a high hardness after curing, and it is not easy to form mottled pits during the surface treatment process, thereby improving the glossiness of the board surface. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Table 1 - Sources of raw materials in the examples and comparative examples of the present application
[0031]
[0032] Examples 1-6
[0033] A UV-resistant aged quartz stone plate comprises methyl methacrylate-methyl methacrylate copolymer, quartz sand, quartz powder, silane coupling agent, curing agent, accelerator, and color paste. Preferably, the quartz sand comprises quartz sand with a mesh number of 8-16 mesh, 26-40 mesh, or 70-120 mesh, the mesh number of the quartz powder is 400 mesh, the curing agent is tert-butyl peroxymaleate, the silane coupling agent is methacrylate-3-(trimethoxysilyl)propyl ester, and solid particles with an average particle size of 0.05 mm are also included, the solid particles are silica rock or shell powder, and the accelerator is JHT8-D (cobalt water). The preparation method thereof is as follows:
[0034] S1, weighing the formula amount of quartz sand, quartz powder and solid particles and mixing them evenly to obtain an aggregate mixture, which is set aside, weighing the formula amount of methyl acrylate-methyl methacrylate copolymer, silane coupling agent, curing agent, accelerator, and color paste and mixing them evenly to obtain a first mixed slurry, which is set aside;
[0035] S2. Pour the aggregate mixture into a stirring pot, add the first mixed slurry under stirring at 10-20 rpm, stir at 10-20 rpm for 1-3 min, and then stir at 30-60 rpm for 2-5 min to obtain a second mixed slurry;
[0036] S3. Inject the second mixed slurry into the mold and spread it evenly, press it under vacuum, the vacuum degree is 0.8-1MPa, and the pressing frequency changes to 25HZ for 5s, 30HZ for 5s, 35HZ for 10s, 45HZ for 20s, 40HZ for 5s, and 35HZ for 5s to obtain a embryonic plate. Put the embryonic plate and the mold into a curing furnace for heating and curing treatment, remove the embryonic plate from the mold, coarsely grind (50-120 mesh), finely grind (300-800 mesh), polish (1000-2500 mesh), and surface treat it with an antifouling liquid, and then coat it with a film to obtain a finished product.
[0037] Table 2 - Components and contents in quartz stone slabs of Examples 1-6 and Comparative Examples 1-2 of the present application
[0038]
[0039]
[0040] Comparative Example 3
[0041] A UV-resistant aged quartz stone plate, wherein each step, reagents used in each step, and process parameters are the same as those in Example 2, except that methyl methacrylate-methyl methacrylate copolymer is replaced by methyl methacrylate.
[0042] Comparative Example 4
[0043] A UV-resistant aged quartz stone plate, wherein each step, reagents used in each step, and process parameters are the same as those in Example 2, except that methyl methacrylate-methyl methacrylate copolymer is replaced by polymethyl methacrylate.
[0044] Comparative Example 5
[0045] A UV-resistant aged quartz stone plate, wherein each step, reagents used in each step, and process parameters are the same as those in Example 2, except that the silane coupling agent is replaced by a titanate coupling agent, and the titanate coupling agent is NDZ-201.
[0046] Comparative Example 6
[0047] A UV-resistant aged quartz stone plate, wherein each step and the reagents and process parameters used in each step are the same as those in Example 2, except that methyl methacrylate-methyl methacrylate copolymer is replaced by an equal amount of quartz resin LY-128TA, and tert-butyl peroxymaleate is replaced by an equal amount of methyl ethyl ketone.
[0048] Performance testing
[0049] 1. Aging resistance test: Performed according to GB / T16422.2-2014 method 3A cycle number 1. The test results are shown in Table 3;
[0050] 2. Hardness test: Hardness test is carried out according to GB / T9966.5-2001 standard. The test results are shown in Table 3.
[0051] 3. Gloss test: Gloss test was carried out according to GB 11942-1989. The test results are shown in Table 3.
[0052] Table 3 - Performance test results of Examples 1-6 and Comparative Examples 1-5 of the present application
[0053]
[0054] Combining the performance test results of Example 6 and Comparative Examples 1-2 in Table 3, it can be seen that Comparative Example 1 does not contain quartz powder and lacks viscosity, so it cannot be pressed into a plate and cannot be made into a plate. Comparative Example 2 does not add quartz sand, resulting in insufficient wear resistance of the product, resulting in a significant reduction in the hardness and gloss of the product.
[0055] Combining the performance test results of Example 2 and Comparative Examples 3-4 and 6 in Table 3, it can be seen that compared with other resins, the present application adopts methyl methacrylate-methyl methacrylate copolymer and the filler in the system to blend with each other. The resulting board is denser and has significantly improved hardness. During the surface polishing process, the shedding of particles can be reduced, the glossiness of the board surface can be improved, and the aging resistance of the board is simultaneously improved.
[0056] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. A UV-resistant aging quartz stone plate, characterized in that: It comprises the following components in parts by weight: Methyl methacrylate-methacrylic acid copolymer: 9 parts to 18 parts; Quartz sand: 35-40 parts; Quartz powder: 25 parts; Silane coupling agent: 0.08-1 part; Curing agent: 0.08-0.25 parts; Accelerator: 0.008-0.03 parts; Color paste: 0.05-0.7 parts; The mesh number of the quartz sand is 6-120 meshes, and the mesh number of the quartz powder is 325-400 meshes; the quartz stone plate also includes 10-20 parts by weight of solid particles, and the solid particles are silica rock or shell powder; When the solid particles are 10 parts by weight of silica rock, the mass ratio of the quartz sand, quartz powder and solid particles is 8:5:2; the quartz sand includes 10 parts by weight of 8-16 mesh, 15 parts by weight of 26-40 mesh, and 15 parts by weight of 70-120 mesh quartz sand; When the solid particles are 20 parts by weight of shell powder, the mass ratio of the quartz sand, quartz powder and solid particles is 7:5:4; the quartz sand includes 5 parts by weight of 8-16 mesh, 15 parts by weight of 26-40 mesh, and 15 parts by weight of 70-120 mesh quartz sand.
2. The UV-resistant aging quartz stone plate according to claim 1, characterized in that: The silane coupling agent is one or more of 3-(trimethoxysilyl)propyl methacrylate, 3-(2;3-epoxypropoxy)propyltrimethoxysilane and gamma-aminopropyltriethoxysilane.
3. The UV-resistant aging quartz stone plate according to claim 1, characterized in that: The curing agent is tert-butyl permaleate.
4. The UV-resistant aging quartz stone plate according to claim 1, characterized in that: The accelerator is JHT8-D.
5. A method for preparing the UV-resistant aged quartz stone slab according to any one of claims 2 to 4, characterized in that: The following steps are involved: S1, weighing quartz sand, quartz powder and solid particles and mixing them evenly to obtain an aggregate mixture, weighing methyl methacrylate-methacrylic acid copolymer, silane coupling agent, curing agent, accelerator and color paste and mixing them evenly to obtain a first mixed slurry; S2, pouring the aggregate mixture into a stirring device, adding the first mixed slurry under stirring conditions, stirring evenly, to obtain a second mixed slurry; S3, injecting the second mixed slurry into the mold and evenly spreading it, pressing it under vacuum to obtain a embryonic plate, placing the embryonic plate and the mold into a curing furnace for heating and curing treatment, demolding, surface treatment of the embryonic plate, and coating to obtain a finished product.
6. The method for preparing a UV-resistant aging quartz stone plate according to claim 5, characterized in that: In S2, the aggregate mixture is poured into a mixing device, and the first mixed slurry is added under stirring at 10-20 rpm, and after stirring at 10-20 rpm for 1-3 min, the mixture is stirred at 30-60 rpm for 2-5 min to obtain a second mixed slurry.
7. The method for preparing a UV-resistant aging quartz stone plate according to claim 5, characterized in that: In S3, the pressing conditions under vacuum are: vacuum degree 0.8-1 MPa, and the pressing frequency changes are 25 Hz for 5 s, 30 Hz for 5 s, 35 Hz for 10 s, 45 Hz for 20 s, 40 Hz for 5 s, and 35 Hz for 5 s.
Citation Information
Patent Citations
Preparation method for novel quartz stone plate