A method for removing fluorine and phosphorus impurities in a Bayer process

Through the evaporation, heat exchange crystallization and causticizing reaction in the Bayer process, the problem of a large amount of solid waste generated by the removal of fluorine and phosphorus impurities in alumina production is solved, achieving efficient utilization of resources and reducing energy consumption, and is suitable for most applications Production conditions in alumina plants.

CN116002731BActive Publication Date: 2024-10-29ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310080708.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-13
Publication Date
2024-10-29
Estimated Expiration
2043-01-13

AI Technical Summary

Technical Problem

The existing technology produces a large amount of solid waste calcium fluoride when removing fluorine and phosphorus impurities during the alumina production process, and has high requirements for evaporators and complex processes, making it difficult to adapt to the production conditions of most alumina plants.

Method used

Using the Bayer process, the caustic alkali is evaporated to a target concentration and then crystallized by heat exchange to obtain a fluorine-phosphorus double salt. Cryolite is then generated through dissolution and causticization reactions to reduce the generation of solid waste and improve resource utilization.

Benefits of technology

It effectively reduces the output of solid waste calcium fluoride, reduces evaporation energy consumption, simplifies the fluoride removal process, improves resource utilization, and has wider adaptability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116002731B_ABST
    Figure CN116002731B_ABST
Patent Text Reader

Abstract

The present application relates to a method for removing fluorine and phosphorus impurities in a Bayer process, and belongs to the technical field of light metal smelting. The method comprises: evaporating a decomposition mother liquor until the caustic soda concentration of the decomposition mother liquor reaches a target concentration; performing heat exchange crystallization on the decomposition mother liquor whose caustic soda concentration reaches the target concentration to obtain a first recycled liquid and a double salt of fluorine and phosphorus; dissolving the double salt of fluorine and phosphorus to obtain a dissolved liquid, adding a regulator to the dissolved liquid for reaction to obtain a reaction liquid and cryolite; adding quicklime to the reaction liquid for causticization to obtain calcium fluoride, calcium phosphate and a second recycled liquid; and by recycling part of the fluoride ions to prepare cryolite, the resource utilization rate is improved, and the output of solid waste calcium fluoride is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of light metal smelting, and in particular to a method for removing fluorine and phosphorus impurities in a Bayer process. Background Art

[0002] Bauxite contains trace elements such as lithium, fluorine, and phosphorus. During the production of alumina, these trace elements are enriched in the production system, affecting the production process, increasing the difficulty of production regulation, and reducing product quality. According to relevant scholars, when the concentration of impurities such as phosphorus and fluorine in the alumina system is too high, on the one hand, scars will form on the surface of the equipment, reducing the heat transfer coefficient, causing difficulty in heat exchange of the equipment and increasing energy consumption. On the other hand, these impurities will precipitate during the evaporation process, making it difficult to evaporate the mother liquor and difficult to increase the caustic soda in the system. At the same time, the presence of fluorine will also accelerate the corrosion of the equipment and have an adverse effect on the equipment.

[0003] In the prior art, such as the Chinese invention patent application CN202110819510.1, a method and system for removing sodium fluoride in the alumina production process is to evaporate the mother liquor to increase the caustic concentration to more than 256g / L, then cool it down to below 80°C, precipitate sodium fluoride scars in the evaporator, and then use hot water to dissolve the scars, discharge the sodium fluoride solution, causticize it, and use calcium to fix fluorine to obtain calcium fluoride and low-concentration alkali solution. This method increases the caustic concentration of the mother liquor to more than 256g / L, which has very high requirements for the evaporator. Many alumina plants do not have such evaporation capabilities. At the same time, crystals are precipitated on the evaporator and need to be dissolved with hot water, which is a complicated process. Finally, a large amount of solid waste calcium fluoride is produced. Summary of the invention

[0004] The present application provides a method for removing fluorine and phosphorus impurities in a Bayer process, so as to improve the problem that a large amount of solid waste calcium fluoride is generated when removing fluorine and phosphorus impurities.

[0005] The present application provides a method for removing fluorine and phosphorus impurities in a Bayer process, the method comprising:

[0006] Evaporating the decomposition mother liquor until the caustic soda concentration of the decomposition mother liquor reaches a target concentration;

[0007] The decomposition mother liquor whose caustic soda concentration reaches the target concentration is subjected to heat exchange crystallization to obtain a first recycled liquid and a double salt of fluorine and phosphorus;

[0008] Dissolving the double salt of fluorine phosphorus to obtain a solution,

[0009] Adding a regulator to the dissolved solution to react, thereby obtaining a reaction solution and cryolite;

[0010] Quicklime is added to the reaction solution for causticization to obtain calcium fluoride, calcium phosphate and a second recycled solution.

[0011] As an optional embodiment, the target concentration is 190-240 g / L.

[0012] As an optional embodiment, the heat exchange target temperature of the heat exchange crystallization is 30-50°C; and / or

[0013] The crystallization precipitation time of the heat exchange crystallization is 3-10h.

[0014] As an optional implementation, the method further includes: recycling the first recycled liquid to the alumina batching process.

[0015] As an optional embodiment, the dissolving temperature is 60-90°C; and / or

[0016] The solid ratio of the dissolving solution is 1.4-4.

[0017] As an optional embodiment, the additive includes an inorganic acid and / or sodium bicarbonate.

[0018] As an optional embodiment, the pH value of the reaction solution is 8-11, and the reaction time is 20-60 minutes.

[0019] As an optional embodiment, the relationship between the molar amount a of the quicklime added, the molar amount b of phosphorus in the reaction solution and the molar amount c of fluorine in the reaction solution satisfies: a=m*b+n*c, wherein the value of m is 1.5-1.8 and the value of n is 0.6-0.8.

[0020] As an optional embodiment, the causticizing temperature is 85-95° C., and the causticizing time is 1.5-2.5 h.

[0021] As an optional implementation, the method further includes: recycling the second recycled liquid to the alumina dilution process.

[0022] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0023] The method provided in the embodiment of the present application improves resource utilization and effectively reduces the output of solid waste calcium fluoride by recycling part of the fluoride ions into the preparation of cryolite. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0026] Figure 1 A flowchart of a method provided in an embodiment of the present application;

[0027] Figure 2 A process diagram of the method provided in an embodiment of the present application. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0029] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0030] The present application proposes a method for removing fluorine and phosphorus impurities from the Bayer process, which uses a crystallization co-precipitation method to remove fluorine and phosphorus from the alumina production system. The method evaporates caustic soda at a low concentration, greatly reducing the energy consumption of evaporation; fluorine-containing crystals are directly precipitated in the mother liquor and can be directly salvaged, simplifying the process of fluorine removal. Fluorine-containing crystals are recycled and reused to produce cryolite, thereby improving resource utilization.

[0031] like Figure 1 As shown, the embodiment of the present application provides a method for removing fluorine and phosphorus impurities in a Bayer process, the method comprising:

[0032] S1. The decomposition mother liquor is evaporated until the caustic soda concentration of the decomposition mother liquor reaches the target concentration;

[0033] In some embodiments, the target concentration is 190-240 g / L. Using a lower target concentration greatly reduces evaporation energy consumption, effectively reduces requirements for evaporators, reduces investment costs, and has wider adaptability.

[0034] S2. The decomposition mother liquor having a caustic soda concentration reaching a target concentration is subjected to heat exchange crystallization to obtain a first recycled solution and a double salt of fluorine and phosphorus;

[0035] In some embodiments, the heat exchange target temperature of the heat exchange crystallization is 30-50° C.; the crystallization precipitation time of the heat exchange crystallization is 3-10 h.

[0036] Specifically, in this embodiment, the decomposition mother liquor is evaporated, and after evaporation to the target caustic soda concentration, the decomposition mother liquor is cooled by heat exchange and sent to the mother liquor tank for crystallization. After the crystals are precipitated, the overflow is returned to the alumina production system, the bottom flow is filtered, and the filtrate is returned to the system together with the overflow.

[0037] S3. dissolving the double salt of fluorine phosphorus to obtain a solution,

[0038] In some embodiments, the dissolution temperature is 60-90°C; and the solid ratio of the dissolving solution is 1.4-4.

[0039] S4. Adding a regulator to the dissolved solution to react to obtain a reaction solution and cryolite;

[0040] In some embodiments, the additive includes an inorganic acid and / or sodium bicarbonate. The pH value of the reaction solution is 8-11, and the reaction time is 20-60 min.

[0041] The reason for controlling the pH value of the reaction solution to 8-11 is that it is conducive to the formation of cryolite structure. If the pH value is too large or too small, it is difficult to obtain the cryolite structure.

[0042] S5. Add quicklime to the reaction solution for causticization to obtain calcium fluoride, calcium phosphate and a second recycling solution.

[0043] In some embodiments, the relationship between the molar amount a of the quicklime added, the molar amount b of phosphorus in the reaction solution, and the molar amount c of fluorine in the reaction solution satisfies: a=m*b+n*c, wherein the value of m is 1.5-1.8, and the value of n is 0.6-0.8.

[0044] The reason for controlling the total molar amount of quicklime added to be the sum of 1.5-1.8 times the molar amount of phosphorus and 0.6-0.8 times the molar amount of fluorine in the solution is to increase the removal rate of fluorine and phosphorus. The disadvantage of taking the total molar amount too small is that the removal rate of fluorine and phosphorus is low, and the disadvantage of taking the total molar amount too large is that excessive quicklime is added, which increases the cost.

[0045] In some embodiments, the causticizing temperature is 85-95° C., and the causticizing time is 1.5-2.5 h.

[0046] S6. Reusing the first recycled liquid to the alumina batching process.

[0047] S7. Reuse the second recycled liquid in the alumina dilution process.

[0048] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0049] Example 1

[0050] Taking a certain alumina plant as an example, the caustic soda concentration of its mother liquor is 146g / L, the fluorine concentration is 0.183g / L, and the phosphorus concentration is 0.13g / L. After evaporation, the caustic soda concentration is 190g / L, the fluorine concentration is 0.238g / L, and the phosphorus concentration is 0.17g / L. It is cooled to 50°C, the reaction time is 8h, the fluorine removal rate is 58%, and the phosphorus removal rate is 62%. Crystals are salvaged. Take 70g of salt precipitation crystals and dissolve them in 280mL of water at 60°C, with a fluorine concentration of 4.2g / L and a phosphorus concentration of 5.3g / L; add hydrochloric acid to adjust the solution pH to 8, react for 40min, filter to obtain 1.60g of solid cryolite, and the fluorine concentration in the filtrate drops to 1.24g / L; add quicklime to the filtrate for causticization, the causticization temperature is 95°C, the amount of quicklime added is a molar ratio of phosphorus to 1.5 and a molar ratio of fluorine to 0.6, the reaction time is 2h, and the fluorine and phosphorus in the solution are completely removed.

[0051] Example 2

[0052] Taking a certain alumina plant as an example, the caustic soda concentration of its mother liquor is 146g / L, the fluorine concentration is 0.183g / L, and the phosphorus concentration is 0.13g / L. After evaporation, the caustic soda concentration is 240g / L, the fluorine concentration is 0.3g / L, and the phosphorus concentration is 0.214g / L. It is cooled to 30°C and the reaction time is 3h. The fluorine removal rate is 71%, and the phosphorus removal rate is 73%. Crystals are salvaged. Take 70g of salt precipitation slag and dissolve it in 122mL of water at 85°C, the phosphorus concentration is 8.5g / L, and the fluorine concentration is 7.5g / L; add hydrochloric acid to adjust the solution pH to 8, the reaction time is 20min, filter to obtain 1.41g of solid cryolite, and the fluorine concentration in the filtrate is reduced to 2.21g / L; add quicklime to the filtrate for causticization, the causticization temperature is 95°C, the amount of quicklime added is the molar ratio of phosphorus to 1.8 and the molar ratio of fluorine to 0.8, the reaction time is 2h, and the fluorine and phosphorus in the solution are completely removed.

[0053] Example 3

[0054] Taking a certain alumina plant as an example, the caustic soda concentration of its mother liquor is 146g / L, the fluorine concentration is 0.183g / L, and the phosphorus concentration is 0.13g / L. After evaporation, the caustic soda concentration is 200g / L, the fluorine concentration is 0.25g / L, and the phosphorus concentration is 0.18g / L. It is cooled to 50°C, the reaction time is 8h, the fluorine removal rate is 60%, and the phosphorus removal rate is 64%. The crystals are salvaged. Take 70g of salt precipitation slag and dissolve it in 122mL of water at 85°C, the phosphorus concentration is 8.0g / L, and the fluorine concentration is 7.5g / L; add sulfuric acid, adjust the solution pH to 11, react for 60min, filter to obtain 0.73g of solid cryolite, and the fluorine concentration in the filtrate is reduced to 3.98g / L; add quicklime to the filtrate for causticization, the causticization temperature is 95°C, the amount of quicklime added is a molar ratio of phosphorus to 1.5 and a molar ratio of fluorine to 0.6, the reaction time is 2h, and the fluorine and phosphorus in the solution are completely removed.

[0055] Example 4

[0056] Taking a certain alumina plant as an example, the caustic soda concentration of its mother liquor is 146g / L, the fluorine concentration is 0.183g / L, and the phosphorus concentration is 0.13g / L. After evaporation, the caustic soda concentration is 200g / L, the fluorine concentration is 0.25g / L, and the phosphorus concentration is 0.18g / L. It is cooled to 40°C, the reaction time is 8h, the fluorine removal rate is 65%, and the phosphorus removal rate is 68%. The crystals are salvaged. Take 70g of salt precipitation slag and dissolve it in 100mL of water at 90℃, the fluorine concentration is 9.05g / L, and the phosphorus concentration is 7.6g / L; add sodium bicarbonate, adjust the solution pH to about 10, react for 60min, filter to obtain 1.40g of solid cryolite, and the fluorine concentration in the filtrate is reduced to 3.24g / L; add quicklime to the filtrate for causticization, the causticization temperature is 95℃, the amount of quicklime added is the molar ratio of phosphorus to 1.5 and the molar ratio of fluorine to 0.6, the reaction time is 2h, and the fluorine and phosphorus in the solution are completely removed.

[0057] Comparative Example 1

[0058] Taking a certain alumina plant as an example, the caustic soda concentration of its mother liquor is 146g / L, the fluorine concentration is 0.183g / L, and the phosphorus concentration is 0.13g / L. After evaporation, the caustic soda concentration is 200g / L, the fluorine concentration is 0.25g / L, and the phosphorus concentration is 0.18g / L. The temperature is lowered to 70°C, the reaction time is 10h, and no crystallization is precipitated.

[0059] Comparative Example 2

[0060] Take a certain alumina plant as an example, the mother liquor has a caustic concentration of 146g / L, a fluorine concentration of 0.183g / L, and a phosphorus concentration of 0.13g / L. After evaporation, the caustic concentration is 200g / L, the fluorine concentration is 0.25g / L, and the phosphorus concentration is 0.18g / L. After cooling to 40°C, the reaction time is 8h, the fluorine removal rate is 65%, and the phosphorus removal rate is 68%. Crystals are salvaged. Take 70g of salt slag, dissolve it in 100mL of water at 90°C, the fluorine concentration is 9.05g / L, and the phosphorus concentration is 7.6g / L; do not adjust the pH value of the solution, the reaction time is 60min, and no solid cryolite is produced; add quicklime to the filtrate for causticization, the causticization temperature is 95°C, the amount of quicklime added is a molar ratio of phosphorus to 1.5 and a molar ratio of fluorine to 0.6, the reaction time is 2h, and the fluorine and phosphorus in the solution are completely removed.

[0061] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0062] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0063] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for removing fluorine and phosphorus impurities in a Bayer process, characterized in that: The method comprises: Evaporating the decomposition mother liquor until the caustic soda concentration of the decomposition mother liquor reaches 190-240 g / L; The decomposition mother liquor whose caustic soda concentration reaches the target concentration is subjected to heat exchange crystallization to obtain the first recycled liquid and the double salt of fluorine and phosphorus, the heat exchange target temperature of the heat exchange crystallization is 40-50° C., and the crystallization precipitation time of the heat exchange crystallization is 3-10 hours; Dissolving the double salt of fluorophosphorus to obtain a solution, wherein the dissolving temperature is 60-90° C.; Adding an inorganic acid and / or sodium bicarbonate to the dissolved solution for reaction to obtain a reaction solution and cryolite; Adding quicklime to the reaction solution for causticization to obtain calcium fluoride, calcium phosphate and a second recycled solution; The pH value of the reaction solution is 8-11, and the reaction time is 20-60 min; The relationship between the molar amount of quicklime added a, the molar amount of phosphorus in the reaction solution b and the molar amount of fluorine in the reaction solution c satisfies: a=m*b+n*c, wherein the value of m is 1.5-1.8, and the value of n is 0.6-0.8; The causticizing temperature is 85-95°C, and the causticizing time is 1.5-2.5h; The decomposition mother liquor has a caustic soda concentration of 146 g / L, a fluorine concentration of 0.183 g / L, and a phosphorus concentration of 0.13 g / L.

2. The method for removing fluorine and phosphorus impurities from the Bayer process according to claim 1, characterized in that: The method further comprises: recycling the first recycled liquid to the alumina batching process.

3. The method for removing fluorine and phosphorus impurities from the Bayer process according to claim 1, characterized in that: The method further comprises: recycling the second recycled liquid to the alumina dilution process.

Citation Information

Patent Citations

  • Method and system for removing sodium fluoride in aluminum oxide production process

    CN113562754A

  • Method for preparing cryolite by using phosphoric acid industry waste gas

    CN109665551A