A kind of expansion tape for lithium battery packaging and preparation method thereof
The expanded tape prepared through co-extrusion technology solves the environmental pollution and reliability problems of the solvent method in the preparation of lithium battery tape, achieves efficient and reliable expansion tape preparation, and meets the electrolyte resistance and filling requirements of lithium battery packaging. .
Patent Information
- Application Number
- CN202211668551.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-24
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-24
AI Technical Summary
The solvent method used in the existing lithium battery tape preparation method has problems such as multiple production processes, large environmental pollution, long-term high temperature resistance to electrolyte solution, dissolution failure, and filling reliability failure.
Co-extrusion technology is used to prepare expansion tape for cylindrical lithium battery packaging, including a protective layer, a core layer and an adhesive layer. It is formed into a film through three-layer co-extrusion on a casting machine. The composition includes polyethylene, polypropylene, thermoplastic polyurethane, thermoplastic Expanding tape of styrene-butadiene rubber and tackifying resin.
It improves production efficiency, enhances electrolyte resistance expansion rate and filling reliability, and overcomes the complex process of the solvent method and the problem of easy dissolution and failure of electrolyte resistance performance.
Smart Images

Figure BDA0004015584310000051 
Figure BDA0004015584310000061 
Figure BDA0004015584310000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium battery tapes, and in particular to an expansion tape for cylindrical lithium battery packaging and a preparation method thereof. Background Art
[0002] During the assembly process of cylindrical lithium batteries, since there is a certain gap between the battery cell and the cylindrical shell, the battery cell needs to be effectively fixed on the cylindrical shell to avoid the battery cell moving due to vibration and impact, resulting in increased internal resistance of the battery or damage to the electrode and other adverse phenomena.
[0003] The existing technology mostly adopts OPS film or TPU film as substrate, and prepares expansion tape by coating pressure-sensitive adhesive layer to fill the gap. Such methods all adopt solvent method to coat adhesive on the above OPS film or TPU film, which has the disadvantages of many production processes, large environmental pollution, and long-term high temperature resistance to electrolyte, resulting in dissolution failure and filling reliability failure.
[0004] Therefore, there is a need for an expandable tape for cylindrical lithium battery packaging that can solve the above problems. Summary of the invention
[0005] An object of the present invention is to provide a new technical solution for expansion tape for cylindrical lithium battery packaging.
[0006] According to a first aspect of the present invention, there is provided an expansion tape for lithium battery packaging, comprising a protective layer, a core layer and an adhesive layer, wherein:
[0007] The protective layer comprises, by weight: 18-30 parts of polyethylene, 12-22 parts of polypropylene, 48-70 parts of thermoplastic polyurethane, 0.1-0.5 parts of an anti-blocking agent, and 0.3-1.5 parts of an antioxidant;
[0008] The core layer comprises, by weight: 72-86 parts of polyethylene, 14-28 parts of thermoplastic polyurethane elastomer and 0.3-1.5 parts of antioxidant;
[0009] The adhesive layer comprises, by weight, 45-65 parts of thermoplastic styrene-butadiene rubber and 35-55 parts of tackifying resin.
[0010] Preferably, the polypropylene is at least one of block copolymer polypropylene or random copolymer polypropylene.
[0011] Preferably, the polyethylene is at least one of LDPE or HDPE.
[0012] Preferably, the thermoplastic polyurethane is at least one of polyester TPU, polyether TPU, polycaprolactone TPU or polybutadiene TPU.
[0013] Preferably, the anti-blocking agent is at least one of modified nano-silicon dioxide, diatomaceous earth or oleic acid amide; the antioxidant is at least one of hindered phenol antioxidants or phosphite antioxidants.
[0014] Preferably, the thermoplastic styrene-butadiene rubber is at least one of SIS, SBS or SEBS block copolymers.
[0015] Preferably, the tackifying resin is at least one of petroleum resin, terpene resin or rosin resin.
[0016] According to a second aspect of the present invention, there is provided a method for preparing the expansion tape for lithium battery packaging as described in any one of the above, comprising the following steps:
[0017] The components of the protective layer, the core layer and the viscous layer are respectively mixed uniformly to obtain a protective layer premix, a core layer premix and a viscous layer premix;
[0018] The protective layer premix, the core layer premix and the viscous layer premix are respectively placed in corresponding barrels of a tape casting machine, and three layers are co-extruded into a film to obtain the expansion tape for cylindrical lithium battery packaging.
[0019] Preferably, the total thickness of the expansion tape is 0.020-0.080 mm, wherein the thickness of the protective layer is 0.010-0.050 mm, the thickness of the core layer is 0.005-0.020 mm, and the thickness of the adhesive layer is 0.002-0.010 mm.
[0020] According to one embodiment of the present disclosure, the protective layer provides strength and expansion performance, and provides protection for the core layer and the adhesive layer; the core layer serves as a connection between the protective layer and the adhesive layer, and provides structural stability through a compatible design with the protective layer and the adhesive layer; the adhesive layer has excellent adhesion and long-term electrolytic resistance, and provides filling reliability.
[0021] The present invention proposes for the first time to use co-extrusion technology to prepare the expansion tape in one step, which has the characteristics of high production efficiency, high electrolyte expansion resistance rate and excellent reliability. It overcomes the shortcomings of the prior art of solvent coating, complex process, easy dissolution failure of long-term electrolyte resistance and poor filling reliability.
[0022] Further features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention. DETAILED DESCRIPTION
[0023] Various exemplary embodiments of the present invention will now be described in detail. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless specifically stated otherwise.
[0024] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.
[0025] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0026] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0027] Example 1
[0028] The expansion tape for lithium battery packaging in this embodiment includes a protective layer, a core layer and an adhesive layer, wherein:
[0029] The protective layer comprises, by weight: 18-30 parts of polyethylene, 12-22 parts of polypropylene, 48-70 parts of thermoplastic polyurethane, 0.1-0.5 parts of an anti-blocking agent, and 0.3-1.5 parts of an antioxidant;
[0030] The core layer comprises, by weight: 72-86 parts of polyethylene, 14-28 parts of thermoplastic polyurethane elastomer and 0.3-1.5 parts of antioxidant;
[0031] The adhesive layer comprises, by weight, 45-65 parts of thermoplastic styrene-butadiene rubber and 35-55 parts of tackifying resin.
[0032] Specifically, the polypropylene is at least one of block copolymer polypropylene or random copolymer polypropylene, preferably block copolymer polypropylene. The polyethylene is at least one of LDPE or HDPE, preferably LDPE.
[0033] The thermoplastic polyurethane is at least one of polyester TPU, polyether TPU, polycaprolactone TPU or polybutadiene TPU, and polyester TPU is preferably used.
[0034] The anti-blocking agent is at least one of modified nano-silicon dioxide, diatomaceous earth or oleic acid amide, preferably modified nano-silicon dioxide; the antioxidant is at least one of hindered phenol antioxidants or phosphite antioxidants. The thermoplastic styrene-butadiene rubber is at least one of SIS, SBS or SEBS block copolymers. The tackifying resin is at least one of petroleum resin, terpene resin or rosin resin, preferably petroleum resin.
[0035] The method for preparing the above-mentioned expansion tape for lithium battery packaging comprises the following steps:
[0036] The components of the protective layer, the core layer and the viscous layer are respectively mixed uniformly to obtain a protective layer premix, a core layer premix and a viscous layer premix;
[0037] The protective layer premix, the core layer premix and the viscous layer premix are respectively placed in corresponding barrels of a tape casting machine, and three layers are co-extruded into a film to obtain the expansion tape for cylindrical lithium battery packaging.
[0038] According to actual use needs, the screw speed can be adjusted to control the layer thickness ratio of each layer of the product, thereby producing products with different layer thicknesses and different overall thicknesses, with high production efficiency. Further, the total thickness of the expansion tape is 0.020-0.080 mm, of which the thickness of the protective layer is 0.010-0.050 mm, the thickness of the core layer is 0.005-0.020 mm, and the thickness of the adhesive layer is 0.002-0.010 mm.
[0039] Through the above technical scheme, the protective layer provides strength and expansion performance, providing protection for the core layer and the adhesive layer; the core layer serves as a connection between the protective layer and the adhesive layer, and provides structural stability through the compatibility design with the protective layer and the adhesive layer; the adhesive layer has excellent adhesion and long-term electrolytic resistance, and provides filling reliability.
[0040] This proposal proposes for the first time to use co-extrusion technology to prepare expansion tape in one step, which has the characteristics of high production efficiency, high electrolyte expansion resistance, and excellent reliability. It overcomes the shortcomings of the solvent coating method used in the prior art, which has complex procedures, long-term electrolyte resistance, easy dissolution and failure, and poor filling reliability.
[0041] Example 2
[0042] An expansion tape for cylindrical lithium battery packaging and a preparation method thereof, comprising the following:
[0043] (1) The components of the protective layer, the core layer and the viscous layer are mixed uniformly according to the proportions in Table 1 to obtain a protective layer premix, a core layer premix and a viscous layer premix;
[0044] (2) The protective layer premix, the core layer premix and the viscous layer premix are respectively placed in a casting machine and co-extruded into a film to obtain an expandable tape with a total thickness of 0.040 mm, a protective layer thickness of 0.025 mm, a core layer thickness of 0.010 mm and a viscous layer thickness of 0.005 mm.
[0045] Example 3
[0046] An expansion tape for cylindrical lithium battery packaging and a preparation method thereof, comprising the following:
[0047] (1) The components of the protective layer, the core layer and the viscous layer are mixed uniformly according to the proportions in Table 1 to obtain a protective layer premix, a core layer premix and a viscous layer premix;
[0048] (2) The protective layer premix, the core layer premix and the viscous layer premix are respectively placed in a casting machine and co-extruded into a film to obtain an expansion tape with a total thickness of 0.050 mm, a protective layer thickness of 0.028 mm, a core layer thickness of 0.012 mm and a viscous layer thickness of 0.010 mm.
[0049] Example 4
[0050] An expansion tape for cylindrical lithium battery packaging and a preparation method thereof, comprising the following:
[0051] (1) The components of the protective layer, the core layer and the viscous layer are mixed uniformly according to the proportions in Table 1 to obtain a protective layer premix, a core layer premix and a viscous layer premix;
[0052] (2) The protective layer premix, the core layer premix and the viscous layer premix are respectively placed in a casting machine and co-extruded into a film to obtain an expansion tape with a total thickness of 0.020 mm, a protective layer thickness of 0.012 mm, a core layer thickness of 0.006 mm and a viscous layer thickness of 0.002 mm.
[0053] Example 5
[0054] An expansion tape for cylindrical lithium battery packaging and a preparation method thereof, comprising the following:
[0055] (1) The components of the protective layer, the core layer and the viscous layer are mixed uniformly according to the proportions in Table 1 to obtain a protective layer premix, a core layer premix and a viscous layer premix;
[0056] (2) The protective layer premix, the core layer premix and the viscous layer premix are respectively placed in a casting machine and co-extruded into a film to obtain an expandable tape with a total thickness of 0.080 mm, a protective layer thickness of 0.050 mm, a core layer thickness of 0.020 mm and a viscous layer thickness of 0.010 mm.
[0057] Comparative Example 1
[0058] The expansion tape is made of OPS substrate coated with pressure-sensitive adhesive, with a thickness of 0.050mm.
[0059] Comparative Example 2
[0060] The expansion tape is made of TPU substrate coated with pressure-sensitive adhesive, with a thickness of 0.050mm.
[0061] Table 1 Components of Examples 2 to 5
[0062]
[0063]
[0064] The above examples and comparative examples were tested in the following manner
[0065] (1) Peel strength: Tested according to Method 1 of GB / T 2792-2014 Test method for peel strength of adhesive tape.
[0066] (2) Total thickness: measured in accordance with GB / T 7125-2014 Test method for thickness of adhesive tape.
[0067] (3) Resistance to electrolyte expansion: Cut the sample into 50 mm × 50 mm specifications, and measure the original length L0, original width W0, and original thickness H0. Lay the sample flat in a bottle, pour the electrolyte into it until the sample is completely immersed, place it at 85°C, observe the sample morphology after 72 hours, and flatten the sample to measure its expansion length L1, width W1, and thickness H1.
[0068] The sample form is represented by the following symbols:
[0069] △: indicates that the sample morphology is observed and the expansion rate can be measured;
[0070] ×: Indicates that the sample morphology was not observed and the expansion rate could not be measured.
[0071] The expansion rate is expressed by the following formula:
[0072] Expansion rate = (L1×W1×H1) / (L0×W0×H0)×100%
[0073] (4) Filling reliability: Prepare a battery cell with expansion tape and install it on the test bench. Apply random and fixed-frequency vibration loads in each direction. The loading sequence should be Z-axis random, Z-axis fixed-frequency, Y-axis random, Y-axis fixed-frequency, X-axis random, and X-axis fixed-frequency. Random vibration is applied for 12 hours in each direction at a frequency of 10 Hz; fixed-frequency vibration is applied for 2 hours in each direction at a frequency of 20 Hz. After the vibration is completed, test the change in its resistance value to evaluate the filling capacity of the expansion tape.
[0074] The filling reliability evaluation is represented by the following symbols:
[0075] ○: The power supply can be detected, and the resistance value changes <10%;
[0076] △: The power supply can be detected, and the resistance value changes ≥ 10%;
[0077] ×: No power supply detected.
[0078] The results of the above tests are shown in Table 2.
[0079] Table 2: Performance parameter table of Examples 2 to 5 and Comparative Examples 1 and 2
[0080]
[0081] Note: In the comparative example, the electrolyte expansion resistance is reflected in the increase in thickness and the contraction in length and width.
[0082] It can be seen from the test results in Table 2 that Example 3 shows an excellent effect and can be used as the best example of the present application. It can be seen from the results shown in Table 2 that the expansion tape for cylindrical lithium battery packaging of the present invention meets the requirements.
[0083] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. An expansion tape for lithium battery packaging, characterized in that: It includes a protective layer, a core layer and an adhesive layer, wherein: The protective layer comprises, by weight: 18-30 parts of polyethylene, 12-22 parts of polypropylene, 48-70 parts of thermoplastic polyurethane, 0.1-0.5 parts of an anti-blocking agent and 0.3-1.5 parts of an antioxidant; the polypropylene is at least one of block copolymer polypropylene or random copolymer polypropylene; the polyethylene is at least one of LDPE or HDPE; the anti-blocking agent is at least one of modified nano-silicon dioxide, diatomaceous earth or oleic acid amide; the antioxidant is at least one of a hindered phenol antioxidant or a phosphite antioxidant; The core layer comprises, by weight: 72-86 parts of polyethylene, 14-28 parts of thermoplastic polyurethane elastomer and 0.3-1.5 parts of antioxidant; the thermoplastic polyurethane is at least one of polyester TPU, polyether TPU or polybutadiene TPU; The adhesive layer comprises, by weight, 45-65 parts of thermoplastic styrene-butadiene rubber and 35-55 parts of tackifying resin.
2. The expandable adhesive tape for lithium battery packaging according to claim 1, characterized in that: The tackifying resin is at least one of petroleum resin, terpene resin or rosin resin.
3. A method for preparing the expandable adhesive tape for lithium battery packaging according to any one of claims 1 to 2, characterized in that: The steps include: The components of the protective layer, the core layer and the viscous layer are respectively mixed uniformly to obtain a protective layer premix, a core layer premix and a viscous layer premix; The protective layer premix, the core layer premix and the viscous layer premix are respectively placed in corresponding material barrels of a tape casting machine, and three layers are co-extruded into a film to obtain the expandable adhesive tape for lithium battery packaging.
4. The preparation method according to claim 3, characterized in that: The total thickness of the expansion tape is 0.020-0.080 mm, wherein the thickness of the protective layer is 0.010-0.050 mm, the thickness of the core layer is 0.005-0.020 mm, and the thickness of the adhesive layer is 0.002-0.010 mm.