Method for utilizing catalytic cracking catalyst residue
By modifying the catalytic cracking catalyst slag, active silicon-aluminum materials are prepared, which are used to prepare catalysts with high activity and excellent heavy oil cracking capabilities, solving the problems of resource waste and molecular sieve quality stability, and improving heavy oil cracking capabilities and Total liquid yield.
Patent Information
- Application Number
- CN202111275094.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The catalytic cracking catalyst slag is not effectively utilized, resulting in waste of resources such as Si and Al. The prior art has shortcomings in the quality stability of molecular sieve and the capacity of heavy oil cracking.
Active silicon aluminum was prepared by slurrying the gum scale, grinding and modifying it in an alkaline solution, aged with an acidic aluminum source and a silicon source at a specific pH and temperature, followed by filtration, drying and washing, and then filtering, drying and washing. Material for the preparation of catalysts with high activity and excellent heavy oil cracking capacity.
The catalyst's efficient heavy oil cracking capacity and total liquid yield are achieved, reducing resource waste and reducing production costs.
Smart Images

Figure BDA0003329824600000111 
Figure BDA0003329824600000121 
Figure BDA0003329824600000122
Abstract
Description
Technical Field
[0001] The invention relates to a method for utilizing catalytic cracking catalyst slag and application of active silicon-aluminum material prepared therefrom. Background Art
[0002] As the catalytic cracking feedstock oil becomes heavier, the catalytic cracking catalyst is required to have stronger and stronger heavy oil cracking ability. Therefore, not only is it required that the main active component Y molecular sieve of the catalytic cracking catalyst has high hydrothermal stability and maintains a suitable distribution of acidic active centers, but also that the matrix component of the catalyst has strong heavy oil macromolecule cracking ability. Usually, the feedstock oil contains heavy oil macromolecules, whose diameter is much larger than the pore diameter of the Y-type molecular sieve and cannot directly enter the molecular sieve pores for cracking. Therefore, the heavy oil molecules need to be pre-cracked on the catalyst matrix to crack into medium-sized molecules, and then the medium-sized molecules enter the molecular sieve pores with stronger acidity to further crack into smaller molecules.
[0003] Catalytic cracking catalyst slag is a waste residue with Al2O3 and SiO2 as main components obtained by sedimentation, filtration and slag cutting of waste water generated in the production of catalytic cracking catalyst, which contains 10-50% by weight of Al2O3, 30-70% by weight of SiO2, 2%-15% of Na2O, and 1%-15% of RE2O3. At present, the slag is mainly discarded directly without being reused, resulting in a waste of resources such as Si and Al. If it is utilized by adopting an industrially feasible and cost-effective technical route, it can not only reduce the environmental protection management pressure of the enterprise, but also help reduce the production cost of the enterprise and improve the economic benefit.
[0004] Zhang Zhimin (Research on the Recycling Technology of Catalytic Cracking Catalyst Slag, Qilu Petrochemical, 2011, 39(3): 219-222) took advantage of the high content of silicon, aluminum and other substances in the catalyst slag and directly used the catalyst slag as the raw material for synthesizing molecular sieves. However, due to the high rare earth content in the slag, the crystallinity of the molecular sieve will be affected. CN102442686B provides a method for preparing a ZSM-5 molecular sieve, which comprises liquidizing a slurry containing a silicon source, an aluminum source, an alkali agent, a template agent and water under crystallization conditions for generating the ZSM-5 molecular sieve, wherein 0.1 to 20 weight % of the silicon source in terms of SiO2 and 0.1 to 60 weight % of the aluminum source in terms of Al2O3 are derived from catalyst slag, the remaining aluminum source is a soluble aluminum salt, and the remaining silicon source is at least one of silica gel, water glass solution, silica sol and silica gel; in the catalyst slag, the content of SiO2 is 20 to 60 weight %, the content of Al2O3 is 15 to 40 weight %, the content of Na2O is 0 to 30 weight %, and the content of rare earth oxide is 0-10 weight %. The method can fully utilize the colloid formed by the silicon and aluminum compounds in the catalyst slag. CN104261425A relates to a method for efficiently utilizing catalytic cracking catalyst residue, which first activates the residue and then synthesizes ultrafine Y-type molecular sieve by hydrothermal crystallization under the action of a structure directing agent. Although the above method can realize the secondary utilization of the residue, it still causes the molecular sieve quality to fluctuate. Once the quality is unstable, a larger amount of residue will be produced. Summary of the invention
[0005] The purpose of the present invention is to provide a method for utilizing catalytic cracking catalyst residue.
[0006] According to one aspect of the present invention, the method for utilizing catalytic cracking catalyst residue provided by the present invention comprises the following steps:
[0007] (1) beating the rubber residue to a solid content of 10 to 30% by weight, grinding it, and then adding an alkaline solution for modification;
[0008] (2) aging the modified slag solution with an acidic aluminum source and a silicon source at a pH of 7 to 11 and 10° C. to 90° C. for 1 to 8 hours; and
[0009] (3) filtering, drying, and washing the dried solid to obtain an active silicon-aluminum matrix material.
[0010] According to some embodiments, the grinding in step (1) is to control the particle size to be D(V, 0.5) ≤ 5 μm, D(V, 0.9) ≤ 15 μm. For example, the particle size is controlled to be D(V, 0.5) ≤ 3 μm, D(V, 0.9) ≤ 7 μm.
[0011] According to some embodiments, in the above step (1), the solid content is controlled to be 10 to 30% by weight, for example, 10 to 20% by weight.
[0012] According to some embodiments, in the above step (1), the alkaline solution is a 10-40 wt % sodium hydroxide or potassium hydroxide solution.
[0013] According to some embodiments, in the above step (1), the amount of the alkaline solution added is 5 to 30% by weight of the alkaline solute to the glue residue.
[0014] According to some embodiments, in step (1), an alkaline solution is added to modify the rubber residue, and the modification conditions are constant temperature stirring reaction at 80-220° C. for 4-24 hours, for example, reaction at 90-160° C. for 4-8 hours.
[0015] According to some embodiments, in step (2), the modified slag solution and the acidic aluminum source and silicon source are simultaneously added to the reactor under high-speed stirring conditions, the molar ratio of the added silicon source to the aluminum source is 9 to 1:1 in terms of oxides (SiO2, Al2O3), and the total amount of the silicon source and the aluminum source added is 0.3 to 1:1 in terms of oxide mass to slag mass.
[0016] The modified slag solution, the acidic aluminum source and the silicon source are added into the reaction kettle simultaneously under the condition of high-speed stirring, and the preferred adding method is parallel flow adding.
[0017] According to some embodiments, the acidic aluminum source in the method is one or more of Al(NO3)3, AlCl3, and Al2(SO4)3; the silicon source is one or more of water glass, acidic silica sol, and alkaline silica sol.
[0018] According to some embodiments, the drying in step (3) is, for example, spray drying.
[0019] According to some embodiments, the dried solid in step (3) is exchange washed with one or more of ammonium salt, dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid, and dilute phosphoric acid as washing liquid, and the washing temperature is 20 to 80° C., for example, 40 to 60° C.; the washing time is 10 to 60 minutes, for example, 20 to 30 minutes; the pH of the washing liquid is 1 to 5, for example, pH 2 to 4.
[0020] According to the method of the present invention, the washed filter cake is dried to obtain an active silicon-aluminum material. Based on the total weight of the silicon-aluminum matrix, the prepared silicon-aluminum material contains 0-3.0 wt. % Na2O, 10-50 wt. % Al2O3, 20-70 wt. % SiO2 and 1-15 wt. % RE2O3. The specific surface area of the active silicon-aluminum material is 200-500 m 2 / g, the pore volume is 0.5~1.0mL / g, and the average pore diameter is 10~40nm.
[0021] According to some embodiments, the active silicon-aluminum material prepared by the method of the present invention contains 0.1-1.5 wt. % Na2O, 20-40 wt. % Al2O3, 30-60 wt. % SiO2 and 2-8 wt. % RE2O3, and the specific surface area of the active silicon-aluminum matrix is 250-400 m 2 / g, the pore volume is 0.5~1.0mL / g, and the average pore diameter is 15~30nm.
[0022] According to another aspect of the present invention, a catalytic cracking catalyst is prepared using a prepared or synthesized silicon-aluminum material as a matrix.
[0023] The catalytic cracking catalyst prepared by the present invention contains 15-50 weight percent of Y-type molecular sieve, 10-50 weight percent of clay, 5-40 weight percent of binder and 2-30 weight percent of active silicon-aluminum material prepared by the present invention, based on its dry weight. The catalyst has higher activity and better coke selectivity.
[0024] According to some embodiments, the catalytic cracking catalyst contains 20-35 wt% of Y-type molecular sieve, 15-45 wt% of clay, 5-25 wt% of binder and 5-25 wt% of the above active silicon-aluminum material.
[0025] The preparation method of the catalytic cracking catalyst of the present invention comprises: mixing and slurrying the clay, the binder and water, adding an inorganic acid to adjust the pH to 2.5-4.0 to obtain a first slurry; mixing the first slurry, an active silicon-aluminum material and a Y-type molecular sieve, and spray drying, roasting and washing the obtained second slurry.
[0026] Optionally, the clay, binder and water are mixed and slurried, and an inorganic acid is added to adjust the pH to 2.5 to 4.0, preferably 2.8 to 3.5, to obtain a first slurry.
[0027] Optionally, the Y-type molecular sieve is selected from one or more of an ultra-stable Y-type molecular sieve, a Y-type molecular sieve containing phosphorus and / or rare earth metals, and an ultra-stable Y-type molecular sieve containing phosphorus and / or rare earth metals; the clay is selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite; the inorganic acid is selected from one or more of hydrochloric acid, nitric acid, sulfuric acid and phosphoric acid; optionally, the binder is selected from one or more of aluminum sol, silica sol, silica-aluminum composite sol, aluminum phosphate sol and acidified pseudo-boehmite.
[0028] Another aspect of the present invention provides an application of the catalytic cracking catalyst of the present invention in the catalytic cracking of heavy oil.
[0029] Another aspect of the present invention provides a catalytic cracking method, which comprises the step of contacting hydrocarbon oil with the catalytic cracking catalyst prepared by the present invention to carry out a reaction.
[0030] Optionally, the conditions for catalytic cracking of the heavy oil include: a temperature of 490-530° C. and a catalyst-oil ratio of 3-8.
[0031] Through the above technical scheme, the catalytic cracking catalyst of the present invention has good heavy oil cracking ability and can significantly improve the yield of total liquid.
[0032] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0033] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0034] The active silicon-aluminum matrix material synthesized by the present invention contains 0-3.0 wt. % Na2O, 10-50 wt. % Al2O3, 20-70 wt. % SiO2 and 1-15 wt. % RE2O3 based on the total weight of the silicon-aluminum matrix, and the specific surface area of the silicon-aluminum matrix is 200-500 m 2 / g, the pore volume is 0.5~1.0mL / g, and the average pore diameter is 10~40nm.
[0035] The catalytic cracking catalyst prepared by using a synthetic silicon-aluminum material as a matrix contains, based on the dry weight of the catalyst, 10 to 50 weight percent of a Y-type molecular sieve, 10 to 50 weight percent of clay, 5 to 40 weight percent of a binder and 2 to 30 weight percent of an active silicon-aluminum material prepared by the present invention, and the catalyst has higher activity and better coke selectivity.
[0036] Among them, RE2O3 refers to rare earth metal oxides, which are well known to those skilled in the art and will not be described in detail here. The catalytic cracking catalyst of the present invention contains active silicon-aluminum materials prepared by using slag, which provides a green way for the effective recycling of silicon, aluminum, rare earth and other resources in the catalyst preparation process. Compared with conventional catalytic cracking catalysts, the catalytic cracking catalyst of the present invention has excellent heavy oil cracking ability and higher total liquid yield.
[0037] In a specific embodiment, the specific surface area of the active silicon-aluminum material is 200 to 350 m 2 / g, the pore volume is 0.7~1.0mL / g, and the average pore diameter is 15~40nm.
[0038] The catalytic cracking catalyst of the present invention may contain 20-45 wt % of Y-type molecular sieve, 15-40 wt % of clay, 10-35 wt % of binder and 5-25 wt % of active silicon-aluminum material prepared by the present invention.
[0039] The method for preparing a catalytic cracking catalyst provided by the present invention comprises: mixing and slurrying the clay, a binder and water, adding an inorganic acid to adjust the pH to 2.5-4.0, to obtain a first slurry; mixing the first slurry, an active silicon-aluminum material and the Y-type molecular sieve, and spray drying, roasting and washing the obtained second slurry.
[0040] The active silicon-aluminum matrix is prepared by the following steps: the slurry is slurried to a solid content of 10-30%, and then finely ground, and then an alkaline solution is added to modify the slag, and the modification conditions are constant temperature stirring reaction at 80-220°C for 4-24 hours. The modified slag solution, the acidic aluminum source, and the silicon source are added to the reactor at the same time under high-speed stirring conditions, the pH is controlled at 7-11, and after aging at 10-90°C for 1-8 hours, it is filtered and dried. The dried solid is washed, and the pH is controlled at 1-5 to obtain an active silicon-aluminum material.
[0041] The method of the invention can realize the recycling of the rubber residue and can prepare a catalytic cracking catalyst with excellent heavy oil cracking activity.
[0042] In some embodiments, the active silicon-aluminum material is prepared by a method comprising the following steps: slurrying the slag to a solid content of 10 to 30%, grinding, and then adding an alkaline solution to modify the slag, and the modification conditions are constant temperature stirring reaction at 80 to 220° C. for 4 to 24 hours. The modified slag solution, the acidic aluminum source, and the silicon source are added to the reactor at the same time under high-speed stirring conditions, the pH is controlled at 7 to 11, and after aging at 10 to 90° C. for 1 to 8 hours, it is filtered and spray-dried. The dried solid is washed and the pH is controlled to be 1 to 5 to obtain the active silicon-aluminum material.
[0043] According to the present invention, the method of grinding the slag is not specifically limited, and can be ball milling, air flow milling, etc. The solution for alkaline modification of the slag can be a mixture of NaOH and KOH solutions or both, and the modification conditions can be constant temperature stirring reaction at 80 to 220° C. for 4 to 24 hours. The modified slag solution and the acidic aluminum source and silicon source are added to the reactor simultaneously under high-speed stirring conditions.
[0044] According to the present invention, the method for preparing a catalytic cracking catalyst may include: mixing and slurrying the clay, the binder and water, adding an inorganic acid to adjust the pH to 2.5-4.0, and obtaining a first slurry; after mixing the first slurry, the active silicon-aluminum material and the Y-type molecular sieve, spray drying, roasting and washing the obtained second slurry; wherein, the time for mixing and slurrying is not specifically limited, for example, it can be 30-120 minutes. Preferably, the solid obtained by drying and optionally roasting is washed and dried, and the type of liquid used for washing is not specifically limited, for example, it can be deionized water, and the drying temperature and time can be selected according to actual needs, which will not be repeated here. Roasting is well known to those skilled in the art, for example, it can be carried out in a muffle furnace or a tubular furnace, the roasting temperature can vary in a large range, preferably 300-650°C, the time can be 1-5 hours, and the roasting atmosphere is not specifically limited, it can be an air atmosphere or an inert atmosphere, and the inert atmosphere can contain an inert gas and / or nitrogen, and the inert gas includes helium, argon, etc.
[0045] In some specific embodiments of the present invention, the method for preparing solid slag may include: beating the slag to a solid content of 10 to 30%, grinding to D(V, 0.5) ≤ 3 μm, D(V, 0.9) ≤ 7 μm, and then adding an alkaline solution to modify the slag, wherein the modification conditions are constant temperature stirring reaction at 80 to 220°C for 4 to 24 hours. The modified slag solution is added to the reactor simultaneously with the acidic aluminum source and the silicon source under high-speed stirring, the pH is controlled at 7 to 11, and after aging at 10°C to 90°C for 1 to 8 hours, it is filtered and dried. The dried solid is washed and the pH is controlled to be 1 to 5 to obtain an active silicon-aluminum material. The drying method may be spray drying, airflow drying, or constant temperature drying, preferably spray drying, and the tail gas temperature of the spray drying is 130 to 200°C, more preferably 140 to 180°C. In the method of the present invention, the active silicon-aluminum matrix is dried and formed and then washed, which can solve the problems of difficulty in washing and filtering Na2O, and is conducive to the preparation of a catalytic cracking catalyst with good cracking activity.
[0046] According to the present invention, the Y-type molecular sieve can be selected from one or more of an ultra-stable Y-type molecular sieve, a Y-type molecular sieve containing phosphorus and / or a rare earth metal, and an ultra-stable Y-type molecular sieve containing phosphorus and / or a rare earth metal. Clay is well known to those skilled in the art, for example, it can be selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite.
[0047] According to the present invention, the binder can be selected from one or more of aluminum sol, silica sol, silica-aluminum composite sol, aluminum phosphate sol and acidified pseudo-boehmite. The binder can be purchased commercially or prepared according to existing methods. For example, the acidified pseudo-boehmite can be prepared according to the methods provided by patents US4010116 and US4206085. Preferably, when the pseudo-boehmite is acidified, the molar ratio of acid to pseudo-boehmite (calculated as alumina) is 0.12 to 0.20. The silica sol can be prepared according to the methods provided by US Patents US3957689 and US3867308.
[0048] The third aspect of the present invention provides an application of the catalytic cracking catalyst prepared by the present invention in the catalytic cracking of heavy oil.
[0049] According to the present invention, the conditions for catalytic cracking of heavy oil may include: a temperature of 490 to 530° C. and a catalyst-to-oil ratio of 3 to 8 by weight.
[0050] Example
[0051] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.
[0052] The slag is obtained from the wastewater generated in the production of catalytic cracking catalysts through sedimentation, filtration and slag cutting operations to obtain the discarded slag.
[0053] The solid content of the slag 1# is 25 wt %. Based on the dry weight of the slag, it contains 9.0 wt % of Na2O, 23.0 wt % of Al2O3, 48.0 wt % of SiO2, and 9.2 wt % of RE2O3;
[0054] The solid content of the slag 2# is 20 wt %. Based on the dry weight of the slag, it contains 13 wt % of Na2O, 38 wt % of Al2O3, 31.0 wt % of SiO2, and 12.1 wt % of RE2O3;
[0055] Kaolin was produced by Suzhou Kaolin Company with a solid content of 72% by weight;
[0056] Pseudo-boehmite was produced by Shandong Aluminum Plant and had a solid content of 62.0 wt%;
[0057] The aluminum oxide content in the aluminum sol is 21.5% by weight;
[0058] Hydrochloric acid was produced by Beijing Chemical Plant with analytical grade and mass concentration of 36%;
[0059] Sodium hydroxide was produced by Beijing Chemical Plant and was analytically pure;
[0060] Aluminum sulfate: 90g Al2O3 / L produced by Sinopec Catalyst Co., Ltd.;
[0061] Water glass: SiO2, 250g / L 3.33 mold produced by Sinopec Catalyst Co., Ltd.;
[0062] The solid content of rare earth ultrastable Y molecular sieve REUSY is 95.8% by weight, and the unit cell constant is In terms of weight percentage, the Na2O content is 1.6% and the RE2O3 content is 17.9%;
[0063] The solid content of ultra-stable Y molecular sieve USY is 94.7% by weight, and the unit cell constant is In terms of weight percentage, the Na2O content is 1.3%;
[0064] The two molecular sieves, REUSY and USY, were added into deionized water in a ratio of 4:3 and mixed and slurried to obtain a molecular sieve mixed slurry with a solid content of 35%.
[0065] Rare earth ultra-stable Y molecular sieve REUSY and ultra-stable Y molecular sieve USY are both produced by Sinopec Catalyst Co., Ltd., and the other reagents are produced by Sinopharm Chemical Reagent Co., Ltd., all of which are analytically pure.
[0066] The ASAP 2405N V1.01 automatic adsorption instrument from Micromeritics of the United States was used, and the low-temperature static nitrogen adsorption capacity method was used. The sample was heated to 1.33×10 -2 The sample was vacuum degassed at 300 °C for 4 h, and the adsorption-desorption isotherm of the sample was measured at 77.4 K using N2 as the adsorption medium. The specific surface area (S BET ), measure the volume of N2 adsorbed by the sample when the relative pressure p / p0=0.98, and convert it into liquid nitrogen volume, i.e., pore volume;
[0067] The average pore size of the samples was determined using the Q / SH 3360-206 method;
[0068] The composition of the samples was determined by X-ray fluorescence spectroscopy (XRF);
[0069] NB / SH / T 0952-2017 was used to determine the micro-reaction index of catalytic cracking catalyst;
[0070] The apparent bulk density of catalytic cracking catalyst was determined using NB / SH / T 0954-2017;
[0071] The pore volume of catalytic cracking catalyst was determined using NB / SH / T 0955-2017;
[0072] NB / SH / T 0964-2017 was used to determine the wear index of catalytic cracking catalyst.
[0073] Preparation Example 1
[0074] 400g of slag 1# was slurried evenly under high-speed stirring conditions, and the solid content of the slurry was 15% by weight. It was ground using a high-speed shearing device, and the particle size was D(V,0.5)=0.5μm, D(V,0.9)=1.4μm. 25g of 20% by weight NaOH solution was added, and the reaction was stirred at a constant temperature of 150℃ for 5h and then cooled to 25℃ to obtain the modified slag slurry. The modified slag slurry was added to the reactor with 123ml aluminum sulfate and 160ml water glass under high-speed stirring conditions, and the pH value was controlled at 10.7. After aging at 60℃ for 4h, it was spray-dried. The dried solid was added to deionized water, where deionized water: solid = 10:1 (weight ratio), and then dilute sulfuric acid was added to adjust the pH of the washing slurry to 2. The washing was exchanged twice under stirring conditions and dried at 120℃ to obtain the active silicon-aluminum material GL-1. The specific surface area is 220m2 / g, the pore volume is 0.65mL / g, and the average pore diameter is 25nm. In terms of weight percentage, the Na2O content is 0.8%, the Al2O3 content is 27.1%, the SiO2 content is 63.3%, the RE2O3 content is 7%, and the solid content is 95.1%.
[0075] Preparation Example 2
[0076] 400g of slag 1# was slurried evenly under high-speed stirring conditions, and the solid content of the slurry was 15%. It was ground using a high-speed shearing device, and the particle size was D(V,0.5)=2.7μm, D(V,0.9)=6.8μm. 75g of 20 wt% NaOH solution was added, and the temperature was lowered to 25℃ after constant temperature stirring at 120℃ for 8h. The modified slag solution was added to the reactor with 171ml of aluminum sulfate and 128ml of water glass under high-speed stirring conditions, and the pH was controlled at 9.8. After aging at 60℃ for 4h, it was filtered and dried. The dried solid was added to deionized water, where deionized water: solid = 10:1 (weight ratio), and then dilute sulfuric acid was added to adjust the pH of the washing slurry to 2. The washing was exchanged twice under stirring conditions, and dried at 120℃ to obtain the active silicon-aluminum material GL-2. The specific surface area is 270m2 / g, the pore volume is 0.72mL / g, and the average pore size is 21nm. In terms of weight percentage, the Na2O content is 0.7%, the Al2O3 content is 30.2%, the SiO2 content is 62.4%, and the RE2O3 content is 7.2%; the solid content is 94.2%
[0077] Preparation Example 3
[0078] 400g of slag 1# was slurried evenly under high-speed stirring conditions, and the solid content of the slurry was 15%. It was ground using a high-speed shearing device, and the particle size was D(V,0.5)=4.2μm, D(V,0.9)=11.9μm. 125g of 20 wt% NaOH solution was added, and the mixture was stirred at a constant temperature of 90℃ for 2h before cooling to room temperature of 25℃. The modified slag solution was added to the reactor with 340ml of aluminum sulfate and 152ml of water glass under high-speed stirring conditions, and the pH was controlled at 8.3. After aging at 60℃ for 4h, it was filtered and dried. The dried solid was added to deionized water, where deionized water: solid = 10:1 (weight ratio), and then dilute sulfuric acid was added to adjust the pH of the washing slurry to 2. The mixture was exchanged and washed twice under stirring conditions, and dried at 120℃ to obtain the active silicon-aluminum material GL-3. The specific surface area is 310m2 / g, the pore volume is 0.8mL / g, and the average pore diameter is 17nm. In terms of weight percentage, the Na2O content is 1.3%, the Al2O3 content is 35.1%, the SiO2 content is 57.5%, the RE2O3 content is 9.3%, and the solid content is 96.7%
[0079] Preparation Example 4
[0080] 500g of slag 2# was slurried evenly under high-speed stirring conditions, and the solid content of the slurry was 15%. It was ground using a high-speed shearing device, and the particle size was D(V,0.5)=1.3μm, D(V,0.9)≤3.8μm. 150g of 20 wt% NaOH solution was added, and the temperature was lowered to 25℃ after constant temperature stirring at 110℃ for 3h. The modified slag solution was added to the reactor with 244ml of aluminum sulfate and 140ml of water glass under high-speed stirring conditions, and the pH was controlled at 7.3. After aging at 40℃ for 8h, it was spray-dried. The dried solid was added to deionized water, where deionized water: solid = 10:1 (weight ratio), and then dilute sulfuric acid was added to adjust the pH of the washing slurry to 2. The active silicon-aluminum material GL-4 was obtained. The specific surface area is 350m2 / g, the pore volume is 0.8mL / g, and the average pore size is 19nm. In terms of weight percentage, the Na2O content is 1.1%, the Al2O3 content is 48.1%, the SiO2 content is 41.1%, the RE2O3 content is 8.1%, and the solid content is 91.2%.
[0081] Preparation Comparative Example 1
[0082] The slurry 1# of the catalytic cracking catalyst was stirred evenly and dried at 120°C for 12 hours, and the solid content of the slurry was 20% by weight. The obtained solid slurry was called JZ-D1.
[0083] The content of Na2O in the slag JZ-D1 is 8.9 wt %, the content of A12O3 is 23.1 wt %, the content of SiO2 is 48.0 wt %, the content of RE2O3 is 9.1 wt %, and the specific surface area is 145 m 2 / g, the pore volume is 0.6mL / g, the average pore diameter is 15nm, and the solid content is 89.5%.
[0084] Examples 1 to 8 are examples of preparing catalytic cracking catalysts, and Comparative Examples 1 to 2 are examples of preparing comparative catalytic cracking catalysts.
[0085] Example 1
[0086] 319g of kaolin, 418g of aluminum sol, 323g of pseudo-boehmite and 1203g of decationized water were added to a pulping tank and pulped for 60 minutes, hydrochloric acid was added to adjust the pH to 3.0, and stirring was continued for 60 minutes to obtain a first slurry; then 137g of the active silica-alumina material GL-1 prepared in Preparation Example 1 was added as a matrix and 1000g of molecular sieve was mixed into a slurry, stirred for 60 minutes, the obtained slurry was spray-dried and formed, calcined at 500°C for 2 hours, and washed twice at 60°C according to water: catalyst = 10:1 (weight ratio), ammonium sulfate 3% by weight of the catalyst, and dried to obtain the catalytic cracking catalyst C1 provided by the present invention.
[0087] Embodiments 2 to 4
[0088] Catalytic cracking catalysts C2, C3 and C4 were prepared by the same method as in Example 1, except that the active silica-alumina material GL-1 in Example 1 was replaced by the same amount of active silica-alumina matrices GL-2, GL-3 and GL-4 in Examples 2 and 3, respectively.
[0089] Comparative Example 1
[0090] The catalytic cracking catalyst DB1 was prepared in the same manner as in Example 1, except that the active silicon-aluminum material GL-1 in Example 1 was replaced by an equal amount of the slag JZ-D1 prepared in Comparative Example 1.
[0091] Comparative Example 2
[0092] The catalytic cracking catalyst DB2 was prepared by the same method as in Example 1, except that no slag was added, 500 g of kaolin, 418 g of aluminum sol, 323 g of pseudo-boehmite and 1170 g of decationized water were added to a pulping tank and pulped for 90 minutes, hydrochloric acid was added to adjust the pH to 3.0, and stirring was continued for 60 minutes to obtain a first slurry; then 1000 g of molecular sieve mixed slurry was added, stirred for 60 minutes, the obtained slurry was spray dried to form, calcined at 500°C for 2 hours, and washed twice at 60°C according to water: catalyst = 10:1 (weight ratio), 3% of the catalyst weight of ammonium sulfate, and dried to obtain the catalytic cracking catalyst DB2 provided by the present invention.
[0093] Test Example 1
[0094] Catalysts C1-C4 and DB1-DB2 were pre-aged in a fixed bed aging device at 800°C and 100% steam for 17 hours, and then evaluated in a small fixed bed reactor. The properties of the reaction raw oil are shown in Table 1. The reaction temperature is 500°C, the catalyst-oil ratio (weight ratio) is 4, and the weight hourly space velocity is 8h -1 .
[0095] Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield;
[0096] Total liquid yield = liquefied gas yield + gasoline yield + diesel yield;
[0097] Coke selectivity = coke yield / conversion rate; the evaluation results are shown in Table 2.
[0098] Table 1 Raw oil properties
[0099]
[0100]
[0101] Table 2 Evaluation results
[0102]
[0103] The results in Table 2 show that, compared with Comparative Example 1, the catalysts C1 to C4 containing an active silica-alumina matrix prepared by Examples 1 to 4 of the present invention have significantly improved conversion rates and significantly reduced heavy oil yields, which indicates that untreated gum residue is not suitable for direct use in the preparation of catalytic cracking catalysts. Compared with Comparative Example 2, the catalysts C1 to C4 containing an active silica-alumina matrix prepared by the present invention have high total yields of liquefied gas, gasoline and diesel, low heavy oil yields, and reduced coke selectivity, indicating that the catalytic cracking catalyst containing an active silica-alumina matrix has a stronger heavy oil cracking ability, increased total liquid yield, and improved coke selectivity.
[0104] Example 5
[0105] 444g of kaolin, 372g of aluminum sol, 323g of pseudo-boehmite and 1141g of decationized water are added to a pulping tank and pulped for 60 minutes, hydrochloric acid is added to adjust the pH to 3.0, and stirring is continued for 60 minutes to obtain a first slurry; then 53g of active silica-alumina matrix GL-1 and 1000g of mixed molecular sieve slurry are added, and the mixture is stirred for 60 minutes. The obtained slurry is spray-dried and formed, and calcined at 500°C for 2 hours, and washed twice at 60°C according to water: catalyst = 10:1 (weight ratio), ammonium sulfate 3% by weight of the catalyst, and dried to obtain the catalytic cracking catalyst C5 provided by the present invention.
[0106] Example 6
[0107] 333g of kaolin, 465g of aluminum sol, 290g of pseudo-boehmite and 1143g of decationized water are added to a pulping tank and pulped for 60 minutes, hydrochloric acid is added to adjust the pH to 3.0, and stirring is continued for 60 minutes to obtain a first slurry; then 159g of active silica-alumina matrix GL-2 and 943g of mixed molecular sieve slurry are added, and the mixture is stirred for 60 minutes. The obtained slurry is spray-dried and formed, and calcined at 500°C for 2 hours, and washed twice at 60°C according to water: catalyst = 10:1 (weight ratio), ammonium sulfate 3% by weight of the catalyst, and dried to obtain the catalytic cracking catalyst C6 provided by the present invention.
[0108] Example 7
[0109] 236g of kaolin, 558g of aluminum sol, 258g of pseudo-boehmite and 1165g of decationized water are added to a pulping tank and pulped for 60 minutes, hydrochloric acid is added to adjust the pH to 3.0, and stirring is continued for 60 minutes to obtain a first slurry; then 258g of active silica-alumina matrix GL-3 and 875g of mixed molecular sieve slurry are added, and the mixture is stirred for 60 minutes. The obtained slurry is spray-dried and formed, and calcined at 500°C for 2 hours. According to the ratio of water to catalyst = 10:1 (weight ratio), ammonium sulfate is added at 3% by weight of the catalyst, and the mixture is washed twice at 60°C and dried to obtain the catalytic cracking catalyst C7 provided by the present invention.
[0110] Example 8
[0111] 458g of kaolin, 419g of aluminum sol, 322g of pseudo-boehmite and 1189g of decationized water are added to a pulping tank and pulped for 60 minutes, hydrochloric acid is added to adjust the pH to 3.0, and stirring is continued for 60 minutes to obtain a first slurry; then 88g of active silica-alumina matrix GL-4 and 875g of mixed molecular sieve slurry are added, and the mixture is stirred for 60 minutes. The obtained slurry is spray-dried and formed, and calcined at 500°C for 2 hours, and washed twice at 60°C according to water: catalyst = 10:1 (weight ratio), ammonium sulfate 3% by weight of the catalyst, and dried to obtain the catalytic cracking catalyst C8 provided by the present invention.
[0112] Test Example 2
[0113] Catalytic cracking catalysts C5-C8 were pre-aged in a fixed bed aging device at 800°C and 100% by volume steam for 17 hours, and then evaluated in a small fixed fluidized bed device. The properties of the reaction feed oil are shown in Table 1. The reaction temperature is 500°C, the catalyst-oil weight ratio is 6, and the weight hourly space velocity is 8h -1 .
[0114] Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield;
[0115] Total liquid yield = liquefied gas yield + gasoline yield + diesel yield;
[0116] Coke selectivity = coke yield / conversion rate. The evaluation results are shown in Table 3.
[0117] Table 3 Evaluation results
[0118]
[0119]
[0120] From the results in Table 3, it can be seen that compared with Comparative Example 2, the catalysts C5 to C8 containing an active silicon-aluminum matrix prepared in the embodiments of the present invention have improved conversion rates, reduced heavy oil yields, increased total liquid yields, and decreased coke selectivity, indicating that the catalytic cracking catalyst containing an active silicon-aluminum matrix has a stronger heavy oil cracking ability and improved coke selectivity.
[0121] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0122] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0123] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for utilizing catalytic cracking catalyst residue, comprising the following steps: (1) Slurrying catalytic cracking catalyst residue to a solid content of 10 to 30% by weight, grinding it, and then adding an alkaline solution for modification; (2) aging the modified slag solution with an acidic aluminum source and a silicon source at a pH value of 7 to 11 and 10° C. to 90° C. for 1 to 8 hours; and (3) filtering, drying, and washing the dried solid to obtain an active silicon-aluminum matrix material; in, The grinding in step (1) is to control the particle size to be D(V,0.5)≤5μm, D(V,0.9)≤15μm; In step (1), the alkaline solution is used to modify the rubber residue, and the modification conditions are constant temperature stirring reaction at 80 to 220° C. for 4 to 24 hours; In step (2), the modified slag solution, the acidic aluminum source and the silicon source are added to the reaction kettle simultaneously under high-speed stirring conditions, the molar ratio of the silicon source to the aluminum source is 9 to 1:1 in terms of oxide, and the total amount of the silicon source and the aluminum source added is 0.3 to 1:1 in terms of oxide to slag mass ratio.
2. The method according to claim 1, wherein: The alkaline solution is a sodium hydroxide or potassium hydroxide solution with a concentration of 10 to 40 weight percent.
3. The method according to claim 1 or 2, wherein: The amount of alkaline solution added is such that the weight ratio of alkaline solute to glue residue is 5 to 30 weight %.
4. The method according to claim 1, wherein: The acidic aluminum source is one or more of Al(NO3)3, AlCl3, and Al2(SO4)3; the silicon source is one or more of water glass, acidic silica sol, and alkaline silica sol.
5. The method according to claim 1, wherein: The dried solid in step (3) is exchange-washed with one or more of ammonium salt, dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid, and dilute phosphoric acid as washing liquid, the washing temperature is 20 to 80° C., the washing time is 10 to 60 minutes, and the pH of the washing liquid is 1 to 5.
6. The method according to any one of claims 1 to 5, wherein: The active silicon-aluminum material obtained by the method contains 0-3.0 wt. % of Na2O, 10-50 wt. % of Al2O3, 20-70 wt. % of SiO2 and 1-15 wt. % of RE2O3, based on the total weight of the silicon-aluminum matrix, and the specific surface area of the active silicon-aluminum material is 200-500 m 2 / g, the pore volume is 0.5~1.0mL / g, and the average pore diameter is 10~40nm.
7. A method for preparing a catalytic cracking catalyst, comprising: Mix clay, a binder and water to make a slurry, add an inorganic acid to adjust the pH value to 2.5-4.0, and obtain a first slurry; After mixing the first slurry, the active silicon-aluminum material according to any one of claims 1 to 6 and the Y-type molecular sieve, the obtained second slurry is spray-dried, calcined and washed.
8. Use of the active silicon-aluminum material obtained by the method according to any one of claims 1 to 6 in the preparation of catalytic cracking catalysts.
9. A catalytic cracking process, comprising the step of contacting hydrocarbon oil with the catalytic cracking catalyst obtained by the process of claim 7.