A propane dehydrogenation catalyst and its preparation method and application

Through the combination of gallium element, Group VIII noble metals and alkali metals and silica-containing composite oxide-based support, a propane dehydrogenation catalyst with low precious metal content was prepared, which solved the problems of catalyst deactivation and environmental pollution, and achieved high conversion rate and selectivity, reducing operating costs.

CN116059999BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111290655.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-02
Publication Date
2024-11-12
Estimated Expiration
2041-11-02

AI Technical Summary

Technical Problem

The existing propane dehydrogenation catalysts have problems such as fast catalyst deactivation, high environmental pollution risk and high cost, which are difficult to meet the growth of the chemical industry's demand for propylene.

Method used

Using gallium elements, Group VIII noble metals and alkali metals/alkali earth metals as catalyst components, combined with a composite oxide-based support containing silica, the catalyst is prepared through impregnation and calcination processes, and the molar ratio is adjusted to achieve high activity under low precious metal content. and highly selective.

Benefits of technology

High propane conversion and propylene selectivity under low Group VIII precious metal conditions are achieved, reducing the risk of catalyst deactivation and environmental pollution, and reducing operating costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003334744800000081
    Figure BDA0003334744800000081
  • Figure BDA0003334744800000091
    Figure BDA0003334744800000091
Patent Text Reader

Abstract

The present invention relates to a propane dehydrogenation catalyst and a preparation method and application thereof, wherein the catalyst contains gallium, a first auxiliary agent, a second auxiliary agent and a composite oxide-based carrier containing silicon dioxide; the first auxiliary agent contains a noble metal of Group VIII, and the second auxiliary agent contains an alkali metal and / or an alkaline earth metal; based on the dry weight of the catalyst, the content of gallium in the catalyst is 0.01-10% by weight, the content of the first auxiliary agent is 0.001-0.045% by weight, and the content of the second auxiliary agent is 0.01-5% by weight; the ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silicon dioxide is 1:(5-30). The content of the noble metal of Group VIII in the propane dehydrogenation catalyst of the present invention is low, but good dehydrogenation performance can still be maintained, and the catalyst has a high raw material conversion rate, as well as selectivity and yield for the target product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a propane dehydrogenation catalyst and a preparation method and application thereof. Background Art

[0002] Propylene is an important basic organic chemical raw material, widely used in the production of polypropylene, acetone, acrylonitrile, propylene oxide, acrylic acid and other chemical products. At present, the supply of propylene mainly comes from the by-products of naphtha cracking to produce ethylene and petroleum catalytic cracking. Since the 1990s, with the continuous increase in the demand for propylene, the traditional propylene production process can no longer meet the chemical industry's demand for propylene, and it is necessary to accelerate the development of other alternative process technologies. Among them, the process of producing propylene by propane dehydrogenation has attracted the most attention. The process technologies for producing propylene by catalytic dehydrogenation of propane that have been industrialized mainly include UOP's Oleflex technology and Lummus' Catofin technology. The Oleflex process uses a moving bed reactor with continuous catalyst regeneration, with Pt-Sn / Al 2 O 3 As catalyst, K or Li is added for modification; Catofin process uses fixed bed reactor with Cr 2 O 3 / Al 2 O 3 The catalyst deactivates quickly and needs to be regenerated every 15 minutes.

[0003] Compared with the above two processes, the fluidized bed dehydrogenation process helps to save investment and operating costs. The fluidized bed dehydrogenation process adopts a single reactor design, the catalyst is continuously regenerated, and the fuel used for catalyst regeneration is directly burned to provide heat, which is conducive to optimizing the heat balance in the system without the need for an additional heating furnace. In addition, non-hydrogen reaction conditions help to increase propane conversion, reduce propane circulation, and reduce compressor power consumption. The FBD fluidized bed dehydrogenation process jointly developed by the Yaroslavl Research Institute of Russia and Snamprogetti Engineering Company of Italy was industrialized in 1964, and the catalyst used was microsphere Cr 2 O 3 / Al 2 O 3 However, there are also problems such as high risk of catalyst environmental pollution and difficulty in treatment. Therefore, it is of great significance to develop a propane dehydrogenation catalyst with high activity, low cost and green environmental protection.

[0004] CN111491728 discloses a catalyst comprising gallium, cerium and a mixed oxide carrier which can be used for the dehydrogenation of hydrocarbons, wherein the gallium oxide in the catalyst is present in an amount ranging from about 0.1 wt % to about 30 wt % in the composition; the cerium oxide is present in an amount ranging from about 0.1 wt % to about 15 wt % in the composition; a promoter selected from platinum, iridium, lanthanum or a mixture thereof is present in an amount ranging from about 0.005 wt % to about 4 wt % in the composition; a promoter selected from Group 1 elements is present in an amount ranging from about 0.05 wt % to about 3 wt % in the composition; and a carrier selected from alumina, silica, zirconia, titania or a mixture thereof is present in an amount ranging from about 60 wt % to about 99 wt % in the composition.

[0005] CN112657492 discloses an Ir-GaOx-based propane dehydrogenation catalyst, which is composed of iridium metal or iridium oxide, gallium oxide and Al 2 O 3 The carrier composition, wherein the iridium content is Al 2 O 3 0.03-1.5wt% of the carrier, gallium content is Al 2 O 3 1-10wt% of the carrier. The catalyst has the advantages of good stability and high propylene selectivity.

[0006] CN105859503A discloses a dehydrogenation catalyst and process for C2-C5 alkanes and short-chain branched alkylbenzenes. The first component of the catalyst is selected from tin, germanium, lead, indium, gallium, thallium or a mixture thereof, preferably gallium (0.3-3.0 wt%), and the second component is selected from a component containing a Group VIII noble metal, preferably Pt (0.0007-0.04 wt%), and loaded with an alkali metal or alkaline earth metal, preferably potassium (0.1-1.0 wt%). The molar ratio of the first component to the Group VIII noble metal is 0.1-1000, preferably 1-500, and optimally 1-200. The carrier is γ-Al 2 O 3 The surface area of ​​the carrier is not less than 100m 2 / g, preferably 115-250m 2 / g, silicon component (0.0-2.0wt%) can be added to improve mechanical properties, and the particle size is 5-500μm. A riser reactor is used.

[0007] CN112135687 discloses a catalyst for catalytically dehydrogenating alkanes to their corresponding alkenes. It is composed of platinum, gallium and optionally potassium on an alumina carrier. Silicon dioxide is preferably added to the catalyst in an amount of 5-10 wt% as a promoter of its performance. It contains 0.5-1.5 wt% Ga, 1-100 ppm Pt and 0.05-0.5 wt% K.2 O. SiO 2 / Al 2 O 3 The use of Pt / Ga as a support for light alkane dehydrogenation catalysts significantly reduces the deactivation of the catalyst during the dehydrogenation process. Summary of the invention

[0008] The purpose of the present invention is to provide a propane dehydrogenation catalyst and a preparation method and application thereof. The propane dehydrogenation catalyst of the present invention can maintain good dehydrogenation performance when the content of Group VIII noble metal is low, has better raw material conversion rate, and selectivity and yield of target product.

[0009] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a propane dehydrogenation catalyst, which contains gallium, a first auxiliary agent, a second auxiliary agent and a composite oxide-based carrier containing silica; the first auxiliary agent contains a noble metal of Group VIII, and the second auxiliary agent contains an alkali metal and / or an alkaline earth metal; based on the dry weight of the catalyst, the content of gallium in the catalyst is 0.01-10% by weight, the content of the first auxiliary agent is 0.001-0.045% by weight, and the content of the second auxiliary agent is 0.01-5% by weight; the ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silica is 1:(5-30); the content of the first auxiliary agent is calculated based on the amount of the noble metal element of Group VIII, and the molar content of the second auxiliary agent is calculated based on the total amount of the alkali metal element and the alkaline earth metal element; the molar content of the composite oxide-based carrier containing silica is calculated based on the amount of silica.

[0010] Optionally, the content of gallium in the catalyst is 1-7% by weight, the content of the first auxiliary agent is 0.001-0.035% by weight, and the content of the second auxiliary agent is 0.5-5% by weight.

[0011] Optionally, the ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silicon dioxide is 1:(6-10), more preferably 1:(7-8).

[0012] Optionally, the silicon dioxide-containing composite oxide-based carrier is a silicon-aluminum composite oxide or a silicon-zirconium composite oxide, and the SiO in the silicon-aluminum composite oxide or the silicon-zirconium composite oxide is based on the dry weight of the silicon-aluminum composite oxide or the silicon-zirconium composite oxide. 2 The content is 0.5-30% by weight, preferably 1-20% by weight.

[0013] Optionally, the specific surface area of ​​the composite oxide-based carrier containing silicon dioxide is 80-350 m 2 / g, pore volume is 0.4-0.8cm 3 / g.

[0014] Optionally, the Group VIII noble metal is selected from one or more of platinum, iridium and palladium, preferably platinum; the alkali metal is selected from one or more of lithium, sodium and potassium, and the alkaline earth metal is selected from one or more of magnesium, barium and calcium.

[0015] The second aspect of the present invention provides a method for preparing the catalyst provided in the first aspect of the present invention, the method comprising: mixing a gallium source, a precursor of a first auxiliary agent, a precursor of a second auxiliary agent and a solvent, contacting the obtained impregnation solution with a composite oxide-based carrier containing silica for impregnation, taking out the impregnated solid and optionally drying and calcining it.

[0016] Optionally, the impregnation conditions include: temperature of 20-70°C, time of 1-10 hours, solid-liquid ratio of 1-3 g / mL;

[0017] The calcination conditions include: a temperature of 600-1100°C and a time of 1-10 hours; preferably, a temperature of 700-850°C and a time of 1-10 hours;

[0018] The drying conditions include: temperature of 30-180° C., time of 1-10 hours, and pressure of 0.01-0.1 MPa; preferably 90-130° C., time of 2-8 hours, and pressure of 0.04-0.09 MPa.

[0019] Optionally, the gallium source is a water-soluble gallium-containing compound, preferably one or more selected from gallium nitrate, gallium chloride, and gallium sulfate;

[0020] The precursor of the first auxiliary agent is a water-soluble compound containing a noble metal element of Group VIII, preferably one or more selected from chloroplatinic acid, ammonium chloroplatinate, platinum chloride, a water-soluble iridium-containing compound and a water-soluble palladium-containing compound;

[0021] The precursor of the second auxiliary agent is a water-soluble compound containing alkali metal and / or alkaline earth metal, preferably one or more selected from potassium nitrate, potassium hydroxide, potassium carbonate and calcium nitrate;

[0022] The solvent is water.

[0023] The third aspect of the present invention provides a method for preparing propylene by dehydrogenating propane, the method comprising: contacting propane with the catalyst provided by the first aspect of the present invention to carry out a dehydrogenation reaction.

[0024] Optionally, the dehydrogenation reaction is carried out in a fixed bed or fluidized bed reactor, and the mass space velocity of the propane is 0.1-15h -1 , the temperature of the dehydrogenation reaction is 500-650℃.

[0025] Through the above technical scheme, the propane dehydrogenation catalyst of the present invention can maintain a high dehydrogenation catalytic activity while containing a low content of Group VIII noble metals, and can be used in a propane dehydrogenation reaction to achieve a high raw material conversion rate, as well as selectivity and yield for the target product.

[0026] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0027] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0028] According to a first aspect of the present invention, there is provided a propane dehydrogenation catalyst, which contains gallium, a first auxiliary agent, a second auxiliary agent and a composite oxide-based carrier containing silica; the first auxiliary agent contains a noble metal element of Group VIII, and the second auxiliary agent contains an alkali metal element and / or an alkaline earth metal element; based on the dry weight of the catalyst, the content of gallium in the catalyst is 0.01-10% by weight, the content of the first auxiliary agent is 0.001-0.045% by weight, and the content of the second auxiliary agent is 0.01-5% by weight; the ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silica is 1:(5-30); the content of the first auxiliary agent is calculated based on the amount of the noble metal element of Group VIII, and the molar content of the second auxiliary agent is calculated based on the total amount of the alkali metal element and the alkaline earth metal element; the molar content of the composite oxide-based carrier containing silica is calculated based on the amount of silica.

[0029] The propane dehydrogenation catalyst of the present invention can achieve a high dehydrogenation catalytic activity while containing a low content of Group VIII noble metals by adjusting the ratio of the molar content of the second auxiliary agent to the molar content of the composite oxide-based carrier containing silicon dioxide to 1:(5-30), and can be used for propane dehydrogenation reaction to achieve a high raw material conversion rate, as well as selectivity and yield for the target product.

[0030] In a specific embodiment of the present invention, preferably, the content of gallium in the catalyst is 1-7% by weight, the content of the first auxiliary agent is 0.001-0.035% by weight, and the content of the second auxiliary agent is 0.5-5% by weight.

[0031] In a specific embodiment of the present invention, preferably, the ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silicon dioxide is 1:(6-10), more preferably 1:(7-8). In this preferred case, the dehydrogenation catalyst has better catalytic activity for propane dehydrogenation and selectivity for the target product.

[0032] According to the present invention, the composite oxide-based carrier containing silicon dioxide is a silicon-aluminum composite oxide or a silicon-zirconium composite oxide. More preferably, based on the dry weight of the silicon-aluminum composite oxide or the silicon-zirconium composite oxide, the SiO 2 The content is 0.5-30% by weight, preferably 1-20% by weight.

[0033] In a specific embodiment of the present invention, the specific surface area of ​​the composite oxide-based carrier containing silicon dioxide is 80-350 m 2 / g, pore volume is 0.4-0.8cm 3 / g. The specific surface area and pore volume of the composite oxide-based carrier containing silicon dioxide in the present invention can be obtained by BET detection. The BET detection method is well known to those skilled in the art and will not be described in detail here.

[0034] In a specific embodiment of the present invention, the Group VIII noble metal is selected from one or more of platinum, iridium and palladium, preferably platinum; the alkali metal is selected from one or more of lithium, sodium and potassium, preferably potassium; the alkaline earth metal is selected from one or more of magnesium, barium and calcium, preferably calcium.

[0035] The second aspect of the present invention provides a method for preparing the propane dehydrogenation catalyst provided in the first aspect of the present invention, the method comprising: mixing a gallium source, a precursor of a first auxiliary agent, a precursor of a second auxiliary agent and a solvent, contacting the obtained impregnation solution with a composite oxide-based carrier containing silica for impregnation, taking out the impregnated solid and optionally drying and calcining it.

[0036] In the method, the feeding amount of each raw material can be adjusted so that, based on the dry weight of the catalyst, the content of gallium in the catalyst is 0.01-10% by weight, the content of the first auxiliary agent is 0.001-0.045% by weight, and the content of the second auxiliary agent is 0.01-5% by weight; the ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the silica-containing composite oxide-based carrier is 1:(5-30).

[0037] In a specific embodiment of the present invention, the conditions for the impregnation include: a temperature of 20-70°C, a time of 1-10 hours, a solid-liquid ratio of 1-3 g / mL, preferably a temperature of 25-55°C, and a solid-liquid ratio of 1.2-2.5 g / mL. Preferably, the method further includes: aging the solid obtained after the impregnation and then calcining, and the aging time is 1-10 hours.

[0038] According to the present invention, calcination is an operation well known to those skilled in the art. In a specific embodiment of the present invention, the calcination conditions include: a temperature of 600-1100°C and a time of 1-10 hours; preferably, a temperature of 700-850°C and a time of 2-8 hours. The calcination can be carried out in equipment conventionally used by those skilled in the art, such as a muffle furnace or a tubular furnace. The present invention does not specifically limit the calcination atmosphere, such as an air atmosphere or an inert atmosphere, and the inert atmosphere may contain nitrogen, argon and other inert gases.

[0039] In a specific embodiment of the present invention, the drying conditions include: temperature of 30-180°C, time of 1-10 hours, pressure of 0.01-0.1MPa; preferably 90-130°C, time of 2-8 hours, pressure of 0.04-0.09MPa. The present invention does not specifically limit the drying method, for example, it can be dried at a constant temperature or vacuum drying, preferably vacuum drying.

[0040] In a specific embodiment of the present invention, the gallium source is a water-soluble gallium-containing compound, preferably selected from one or more of gallium nitrate, gallium chloride, and gallium sulfate; the precursor of the first auxiliary agent is a water-soluble compound containing a noble metal element of Group VIII, preferably selected from one or more of chloroplatinic acid, ammonium chloroplatinate, platinum chloride, a water-soluble iridium-containing compound, and a water-soluble palladium-containing compound; the precursor of the second auxiliary agent is a water-soluble alkali metal and / or alkaline earth metal-containing compound, selected from one or more of potassium nitrate, potassium hydroxide, potassium carbonate, and calcium nitrate. The solvent may be water.

[0041] The third aspect of the present invention provides a method for producing olefins by dehydrogenating propane, the method comprising: contacting propane with the catalyst provided by the first aspect of the present invention to carry out a dehydrogenation reaction.

[0042] The propane dehydrogenation catalyst of the present invention is particularly suitable for dehydrogenation reactions in fixed bed or fluidized bed reactors. Since it has a lower Group VIII noble metal content, it can effectively avoid excessive Group VIII noble metal loss caused by catalyst wear in the fluidized bed, and can still maintain relatively good catalytic activity and selectivity for the target product.

[0043] In one embodiment of the present invention, the dehydrogenation reaction is carried out in a fixed bed or fluidized bed reactor, and the mass space velocity of propane is 0.1-15h -1 , the temperature of the dehydrogenation reaction is 500-650℃.

[0044] The present invention is further described below by way of examples, but the present invention is not limited thereto. The raw materials used in the present invention are commercially available unless otherwise specified.

[0045] The composition of each element in the catalyst of the present invention is measured by ICP-OES method.

[0046] Examples 1-8 and Comparative Examples 1-3

[0047] Gallium nitrate, chloroplatinic acid (H 2 PtCl 6 ), potassium nitrate and deionized water to obtain an impregnation solution; at 20°C and a liquid-to-solid ratio of 1.2 g / mL, the carrier is impregnated with the impregnated solution, the impregnated solid is rotary evaporated to dryness at 75°C and a vacuum degree of -0.08 MPa, then dried at 120°C for 12 h, and finally calcined in a muffle furnace at 750°C for 4 h to obtain a propane dehydrogenation catalyst. The composition of the catalyst is shown in Table 1.

[0048] The carrier in Examples 1-8 and Comparative Examples 1 and 2 is a silicon-aluminum composite oxide, wherein SiO 2 The content is 5% by weight and the specific surface area is 250m 2 / g, pore volume is 0.75cm 3 / g. The carrier in Comparative Example 3 is alumina, and its specific surface area is 250m 2 / g, pore volume is 0.75cm 3 / g.

[0049] In the microreactor, 2 mL of catalyst was loaded, propane was used as the raw material, and the mass space velocity of propane feed was 7.0 h-1 at 620 °C and 0.1 MPa. -1 The reaction was carried out under the conditions of , and propane was introduced for 5 min to sample. The propane conversion rate and propylene selectivity were calculated, and the carbon content in the catalyst after the reaction was tested. The conversion rate, propylene selectivity and yield of the propane dehydrogenation reaction are shown in Table 1.

[0050] Table 1

[0051]

[0052]

[0053] As can be seen from Table 1, the propane dehydrogenation catalyst of the present invention has a high propane conversion rate, propylene selectivity and yield. Moreover, when the ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silica is preferably 1:(6-10), the propane conversion rate, propylene selectivity and yield are higher. Further, when the ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silica is preferably 1:(7-8), the propane conversion rate, propylene selectivity and yield are further higher.

[0054] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0055] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0056] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A propane dehydrogenation catalyst, comprising gallium, a first auxiliary agent, a second auxiliary agent and a composite oxide-based carrier containing silicon dioxide; the first auxiliary agent comprises a noble metal element of Group VIII, and the second auxiliary agent comprises an alkali metal element and / or an alkaline earth metal element; Based on the dry weight of the catalyst, the content of gallium in the catalyst is 0.01-10% by weight, the content of the first auxiliary agent is 0.001-0.045% by weight, and the content of the second auxiliary agent is 0.01-5% by weight; the ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silicon dioxide is 1:(5-30); the content of the first auxiliary agent is calculated based on the amount of noble metal elements of Group VIII, and the molar content of the second auxiliary agent is calculated based on the total amount of alkali metal elements and alkaline earth metal elements; the molar content of the composite oxide-based carrier containing silicon dioxide is calculated based on the amount of silicon dioxide.

2. The catalyst according to claim 1, wherein The content of gallium in the catalyst is 1-7% by weight, the content of the first auxiliary agent is 0.001-0.035% by weight, and the content of the second auxiliary agent is 0.5-5% by weight.

3. The catalyst according to claim 1, wherein The ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silicon dioxide is 1:(6-10).

4. The catalyst according to claim 3, wherein The ratio of the molar content of the second auxiliary agent in the catalyst to the molar content of the composite oxide-based carrier containing silicon dioxide is 1:(7-8).

5. The catalyst according to claim 1, wherein The silicon dioxide-containing composite oxide-based carrier is a silicon-aluminum composite oxide or a silicon-zirconium composite oxide. The content of SiO2 in the silicon-aluminum composite oxide or the silicon-zirconium composite oxide is 0.5-30% by weight based on the dry weight of the silicon-aluminum composite oxide or the silicon-zirconium composite oxide.

6. The catalyst according to claim 5, wherein The content of SiO2 in the silicon-aluminum composite oxide or the silicon-zirconium composite oxide is 1-20 wt % based on the dry weight of the silicon-aluminum composite oxide or the silicon-zirconium composite oxide.

7. The catalyst according to claim 1, wherein The specific surface area of ​​the composite oxide-based carrier containing silicon dioxide is 80-350 m 2 / g, pore volume is 0.4-0.8cm 3 / g.

8. The catalyst according to claim 1, wherein The Group VIII noble metal is selected from one or more of platinum, iridium and palladium; the alkali metal is selected from one or more of lithium, sodium and potassium; and the alkaline earth metal is selected from one or more of magnesium, barium and calcium.

9. The catalyst according to claim 8, wherein The Group VIII noble metal is platinum.

10. A method for preparing the catalyst according to any one of claims 1 to 9, the method comprising: A gallium source, a precursor of a first auxiliary agent, a precursor of a second auxiliary agent and a solvent are mixed, and the obtained impregnation solution is contacted with a composite oxide-based support containing silicon dioxide for impregnation, and the impregnated solid is taken out and optionally dried and calcined.

11. The method according to claim 10, wherein: The impregnation conditions include: temperature of 20-70°C, time of 1-10 hours, solid-liquid ratio of 1-3 g / mL; The calcination conditions include: a temperature of 600-1100° C. and a time of 1-10 hours; The drying conditions include: temperature of 30-180° C., time of 1-10 hours, and pressure of 0.01-0.1 MPa.

12. The method according to claim 11, wherein: The calcination conditions include: a temperature of 700-850°C and a time of 1-10 hours; The drying conditions include: temperature of 90-130° C., time of 2-8 hours, and pressure of 0.04-0.09 MPa.

13. The method according to claim 10, wherein: The gallium source is a water-soluble gallium-containing compound; The precursor of the first auxiliary agent is a water-soluble compound containing a noble metal element of Group VIII; The precursor of the second auxiliary agent is a water-soluble compound containing alkali metals and / or alkaline earth metals; The solvent is water.

14. The method according to claim 13, wherein: The gallium source is selected from one or more of gallium nitrate, gallium chloride and gallium sulfate; The precursor of the first auxiliary agent is selected from one or more of chloroplatinic acid, ammonium chloroplatinate, platinum chloride, a water-soluble iridium-containing compound and a water-soluble palladium-containing compound; The precursor of the second auxiliary agent is selected from one or more of potassium nitrate, potassium hydroxide, potassium carbonate and calcium nitrate.

15. A method for preparing propylene by dehydrogenating propane, the method comprising: Propane is contacted with the catalyst according to any one of claims 1 to 9 to carry out a dehydrogenation reaction.

16. The method according to claim 15, wherein: The dehydrogenation reaction is carried out in a fixed bed or fluidized bed reactor, and the mass space velocity of the propane is 0.1-15h -1 , the temperature of the dehydrogenation reaction is 500-650℃.