A 3D vehicle glass surface coating process

Through magnetron sputtering coating technology, high refractive index and low refractive index layers are plated on the surface of 3D vehicle-mounted glass, and combined with the anti-fingerprint layer, the problems of insufficient process stability and poor anti-fingerprint performance in the prior art are solved, and the problem of insufficient anti-fingerprint performance is achieved. 3D automotive glass surface coating process with excellent optical reflection resistance and fingerprint resistance.

CN116083866BActive Publication Date: 2024-12-06凯盛科技股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310028707.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-12-06
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

The AR coating process of existing 3D vehicle-mounted glass is not stable enough, has difficulty in controlling, and has poor fingerprint resistance, which cannot meet the market's demand for optical reflection resistance and fingerprint resistance.

Method used

By using magnetron sputtering coating technology, high-refractive index layer, low-refractive index layer and anti-fingerprint layer are sequentially plating on the surface of 3D vehicle-mounted glass, TiO2, SiO2, Nb2O5, ZrO, SiO2, AlF3, titanium powder and polytetrafluoro Target materials such as ethylene powder combine with argon and nitrogen sputtering atmosphere to form a composite coating layer to improve optical performance and fingerprint resistance.

Benefits of technology

It realizes the low reflectivity and high fingerprint resistance of the surface of 3D vehicle-mounted glass, enhances the wipe resistance and water and oil resistance of the coating, and meets the market's high-performance demand for 3D vehicle-mounted glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004045762970000061
    Figure BDA0004045762970000061
Patent Text Reader

Abstract

The invention discloses a 3D vehicle glass surface coating process, which belongs to the field of vehicle glass technology, and comprises glass base surface pretreatment, vacuuming, pre-sputtering and sputtering coating processes. During the sputtering coating process, a high refractive index layer, a low refractive index layer and an anti-fingerprint layer are sequentially plated from the inside to the outside on the coating base surface of the 3D vehicle glass. The invention forms an optical reflection resistant layer by alternately arranging the high refractive index layer and the low refractive index layer. The optical reflection resistant layer can effectively reduce the reflected light of external light on the surface of the 3D vehicle glass. In the coating process of the anti-fingerprint layer, titanium and polytetrafluoroethylene are used as mixed target materials, and nitrogen and argon are used as sputtering atmospheres for magnetron sputtering, so that an anti-fingerprint coating of titanium nitride and polytetrafluoroethylene is formed on the surface of the 3D vehicle glass. The anti-fingerprint coating has good water and oil resistance properties and can effectively prevent fingerprints from contaminating the surface of the 3D vehicle glass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vehicle-mounted glass, and in particular relates to a 3D vehicle-mounted glass surface coating process. Background Art

[0002] As trends such as automobile electrification, intelligence, and the Internet are increasingly penetrating and developing in the automotive market, the demand for 3D automotive glass for mid-to-high-end automotive touch screens is growing rapidly, and 3D automotive glass is becoming a blue ocean in the automotive glass market.

[0003] The production process of 3D automotive glass includes cutting - CNC1 (glass milling) - hot bending - CNC2 - polishing - silk screen printing / yellow light - coating - packaging. Among them, the coating process is the key process in the manufacturing of 3D automotive glass. The surface of 3D automotive glass needs to be coated with AR coating (anti-reflective coating) and AF coating (anti-fingerprint coating). The glass surface coating technology includes sol-gel coating, magnetron sputtering coating, and chemical vapor deposition coating.

[0004] In the existing AR coating process, a roller coating process or a chemical vapor deposition coating process is generally used. The prepared AR coated glass is formed by a porous SiO2 sol, and the film layer shows a dark blue-purple color. Chinese patent CN101885586B discloses a method for preparing an anti-reflection film on the surface of photovoltaic glass, which includes the following steps: preparing an inorganic-organic hybrid silica sol: coating: hydrophobic treatment: curing treatment. Its advantage is that the film-base bonding between the anti-reflection film and the substrate photovoltaic glass is strong, thereby improving the wipe resistance of the anti-reflection film on the surface of the coated photovoltaic glass. Although the production cost of the anti-reflection film prepared by the sol-gel method is low, the process stability is insufficient and the control is very difficult. Summary of the invention

[0005] The purpose of the present invention is to provide a 3D automotive glass surface coating process. The present invention intends to adopt a magnetron sputtering coating process. Magnetron sputtering coating uses energetic particles to bombard the target material, transfer part of the energy to the target material atoms, and the target material atoms are sputtered out from the target material and deposited on the surface of the substrate to form a thin film. Magnetron sputtering coating is divided into DC magnetron sputtering, medium frequency magnetron sputtering, and radio frequency magnetron sputtering. Magnetron sputtering coated glass is often used in high-end fields. In addition to electrochromic films, it can also be used to prepare common glass surface functional films such as photothermal control films and anti-reflection films. The present invention aims to provide an overall coating process for AR coating and AF coating on the surface of 3D automotive glass by improving the magnetron sputtering coating process, and finally obtain a 3D automotive glass with excellent optical reflection resistance and anti-fingerprint performance to solve the problems in the background technology.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A 3D vehicle glass surface coating process comprises the following steps:

[0008] S1. Vacuuming: Place the 3D automotive glass on the sputtering sample stage of the coating chamber of the magnetron sputtering deposition system, and adjust the vacuum degree in the coating chamber to 0.0035-0.005Pa;

[0009] S2. Pre-sputtering: Under room temperature, the target-substrate distance of the magnetron sputtering deposition system is adjusted to 70-80 mm, the sputtering atmosphere is a high-purity protective gas, the sputtering pressure is 1.2-1.4 Pa, the target power is 85-110 W, and the sputtering time is 5-8 min to complete the pre-sputtering of the 3D automotive glass;

[0010] S3. Sputtering coating: On the coating base surface of the 3D automotive glass, a high refractive index layer, a low refractive index layer and an anti-fingerprint layer are coated in sequence from the inside to the outside. The sputtering pressure is adjusted to 1.0-1.2Pa, the target power is 70-95W, and the sputtering time is 55-85min. After the sputtering is completed, it is cooled to room temperature to obtain a composite layer coated glass, completing the surface coating process of the 3D automotive glass.

[0011] Furthermore, the protective gas is argon or nitrogen.

[0012] Furthermore, the target material of the high refractive index layer is one of TiO2, Nb2O5 and ZrO, and the coating thickness of the high refractive index layer is 30nm-75nm.

[0013] Furthermore, the target material of the low refractive index layer is one of SiO2 and AlF3, and the coating thickness of the low refractive index layer is 35nm-90nm.

[0014] Furthermore, the target material of the anti-fingerprint layer is a mixed target material, and the preparation process of the mixed target material is as follows: titanium powder and polytetrafluoroethylene powder are fully stirred and mixed in a mass ratio of 1.25-1.3:1, and then pressed into blocks to obtain the mixed target material.

[0015] Furthermore, the coating thickness of the anti-fingerprint layer is 45nm-150nm.

[0016] Furthermore, the 3D automotive glass needs to be pretreated before coating: the coated base surface of the 3D automotive glass is ultrasonically cleaned for 15 minutes using anhydrous ethanol, then ultrasonically cleaned for 15 minutes using deionized water, and then placed in a drying room at 80°C for 30 minutes to complete the pretreatment of the 3D automotive glass.

[0017] Beneficial effects of the present invention:

[0018] The present invention provides a 3D vehicle glass surface coating process, in which an optical reflection resistant layer is formed by alternating high refractive index layers and low refractive index layers, and the optical reflection resistant layer can effectively reduce the reflected light of external light on the surface of the 3D vehicle glass; in the coating process of the anti-fingerprint layer, titanium and polytetrafluoroethylene are used as mixed target materials, and nitrogen and argon are used as sputtering atmospheres for magnetron sputtering, so as to form an anti-fingerprint coating of titanium nitride and polytetrafluoroethylene on the surface of the 3D vehicle glass, and the anti-fingerprint coating has good water and oil resistance and can effectively prevent fingerprints from contaminating the surface of the 3D vehicle glass. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Example 1

[0021] Target preparation and selection:

[0022] The target material of the high refractive index layer is TiO2;

[0023] The target material of the low refractive index layer is SiO2;

[0024] The target material of the anti-fingerprint layer is a mixed target material. The preparation process of the mixed target material is as follows: titanium powder and polytetrafluoroethylene powder are fully stirred and mixed in a mass ratio of 1.25:1 and then pressed into blocks.

[0025] Example 2

[0026] Target preparation and selection:

[0027] The target material of the high refractive index layer is Nb2O5;

[0028] The target material of the low refractive index layer is SiO2;

[0029] The target material of the anti-fingerprint layer is a mixed target material. The preparation process of the mixed target material is as follows: titanium powder and polytetrafluoroethylene powder are fully stirred and mixed in a mass ratio of 1.25:1 and then pressed into blocks.

[0030] Example 3

[0031] Target preparation and selection:

[0032] The target material of the high refractive index layer is ZrO;

[0033] The target material of the low refractive index layer is AlF3;

[0034] The target material of the anti-fingerprint layer is a mixed target material. The preparation process of the mixed target material is as follows: titanium powder and polytetrafluoroethylene powder are fully stirred and mixed in a mass ratio of 1.3:1 and then pressed into blocks.

[0035] Example 4

[0036] A 3D vehicle glass surface coating process comprises the following steps:

[0037] S1. Pretreatment: The coated base surface of the 3D automotive glass is ultrasonically cleaned for 15 minutes using anhydrous ethanol, then ultrasonically cleaned for 15 minutes using deionized water, and then dried in a drying room at 80°C for 30 minutes to complete the pretreatment of the 3D automotive glass;

[0038] S2. Vacuuming: Place the 3D automotive glass on the sputtering sample stage of the coating chamber of the magnetron sputtering deposition system, and adjust the vacuum degree in the coating chamber to 0.0035 Pa;

[0039] S3, pre-sputtering: Under room temperature conditions, the target-substrate distance of the magnetron sputtering deposition system was adjusted to 70 mm, the sputtering atmosphere was high-purity argon, the sputtering pressure was 1.2 Pa, the target power was 85 W, and the sputtering time was 5 min, completing the pre-sputtering of the 3D automotive glass;

[0040] S4. Sputtering coating: on the coating base surface of the 3D automotive glass, a 30nm high refractive index layer, a 35nm low refractive index layer and a 45nm anti-fingerprint layer are coated in sequence from the inside to the outside. The target materials of the corresponding layers are determined according to Example 1. The sputtering gas pressure is adjusted to 1.0Pa, the target power is 70W, and the sputtering time is 55min. After the sputtering is completed, it is cooled to room temperature to obtain a composite layer coated glass, thereby completing the surface coating process of the 3D automotive glass.

[0041] Example 5

[0042] A 3D vehicle glass surface coating process comprises the following steps:

[0043] S1. Pretreatment: The coated base surface of the 3D automotive glass is ultrasonically cleaned for 15 minutes using anhydrous ethanol, then ultrasonically cleaned for 15 minutes using deionized water, and then dried in a drying room at 80°C for 30 minutes to complete the pretreatment of the 3D automotive glass;

[0044] S2. Vacuuming: Place the 3D automotive glass on the sputtering sample stage of the coating chamber of the magnetron sputtering deposition system, and adjust the vacuum degree in the coating chamber to 0.0045 Pa;

[0045] S3, pre-sputtering: Under room temperature conditions, the target-substrate distance of the magnetron sputtering deposition system was adjusted to 75 mm, the sputtering atmosphere was high-purity nitrogen, the sputtering pressure was 1.3 Pa, the target power was 95 W, and the sputtering time was 7 min, completing the pre-sputtering of the 3D automotive glass;

[0046] S4. Sputtering coating: on the coating base surface of the 3D automotive glass, a 65nm high refractive index layer, a 45nm low refractive index layer and an 85nm anti-fingerprint layer are coated in sequence from the inside to the outside. The target materials of the corresponding layers are determined according to Example 2. The sputtering gas pressure is adjusted to 1.1Pa, the target power is 80W, and the sputtering time is 75min. After the sputtering is completed, it is cooled to room temperature to obtain a composite layer coated glass, thereby completing the surface coating process of the 3D automotive glass.

[0047] Example 6

[0048] A 3D vehicle glass surface coating process comprises the following steps:

[0049] S1. Pretreatment: The coated base surface of the 3D automotive glass is ultrasonically cleaned for 15 minutes using anhydrous ethanol, then ultrasonically cleaned for 15 minutes using deionized water, and then dried in a drying room at 80°C for 30 minutes to complete the pretreatment of the 3D automotive glass;

[0050] S2. Vacuuming: Place the 3D automotive glass on the sputtering sample stage of the coating chamber of the magnetron sputtering deposition system, and adjust the vacuum degree in the coating chamber to 0.005 Pa;

[0051] S3, pre-sputtering: Under room temperature conditions, the target-substrate distance of the magnetron sputtering deposition system was adjusted to 80 mm, the sputtering atmosphere was high-purity nitrogen, the sputtering pressure was 1.4 Pa, the target power was 110 W, and the sputtering time was 8 min to complete the pre-sputtering of the 3D automotive glass;

[0052] S4. Sputtering coating: on the coating base surface of the 3D automotive glass, a 75nm high refractive index layer, a 90nm low refractive index layer and a 150nm anti-fingerprint layer are coated in sequence from the inside to the outside. The target materials of the corresponding layers are determined according to Example 3. The sputtering gas pressure is adjusted to 1.2Pa, the target power is 95W, and the sputtering time is 85min. After the sputtering is completed, it is cooled to room temperature to obtain a composite layer coated glass, thereby completing the surface coating process of the 3D automotive glass.

[0053] The performance test of the surface-coated 3D vehicle-mounted glass prepared in Examples 4 to 6 was carried out, and the test process was as follows. The test results are shown in Table 1:

[0054] Reflectivity test: According to the distribution characteristics of each wavelength band of sunlight disclosed in GBT2680-1994, the reflectivity of each embodiment and comparative example sample was tested;

[0055] Anti-fingerprint performance test: The surface cleanliness of 3D automotive glass before and after coating is measured using the SITA surface cleanliness meter. The anti-fingerprint performance of 3D automotive glass is characterized mainly by detecting pollutants such as grease and fingerprints. The SITA surface cleanliness meter uses RFU values ​​(Relative Fluorescence Units) to indicate the degree of cleanliness. RFU is the relative fluorescence intensity value. The larger the RFU value, the higher the content of pollutants on the surface of the 3D automotive glass. The specific detection process is as follows:

[0056] The glass samples include surface-coated 3D automotive glass prepared in Examples 4 to 6 and uncoated 3D automotive glass. There are six groups of samples in total, each group has three glass samples, ten test points are selected on the surface of each glass sample, the test points are pressed with fingers, and the RFU value of each test point of each group of glass samples is detected by an instrument, and the instrument automatically calculates the average value.

[0057] Table 1

[0058]

[0059] It can be seen from Table 1 that the coating structure on the surface of the 3D vehicle glass prepared by the 3D vehicle glass surface coating process provided by the present invention has a lower reflectivity and RFU value. The present invention provides a coating process for 3D vehicle glass with excellent optical reflection resistance and anti-fingerprint performance.

[0060] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0061] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A 3D vehicle glass surface coating process, characterized in that: The following steps are involved: S1. Vacuuming: Place the 3D automotive glass on the sputtering sample stage of the coating chamber of the magnetron sputtering deposition system, and adjust the vacuum degree in the coating chamber to 0.0035-0.005Pa; S2. Pre-sputtering: Under room temperature, the target-substrate distance of the magnetron sputtering deposition system is adjusted to 70-80 mm, the sputtering atmosphere is a high-purity protective gas, the sputtering pressure is 1.2-1.4 Pa, the target power is 85-110 W, and the sputtering time is 5-8 min to complete the pre-sputtering of the 3D automotive glass; S3, sputtering coating: on the coating base surface of 3D automotive glass, a high refractive index layer, a low refractive index layer and an anti-fingerprint layer are coated in sequence from the inside to the outside, the sputtering pressure is adjusted to 1.0-1.2Pa, the target power is 70-95W, and the sputtering time is 55-85min. After the sputtering is completed, it is cooled to room temperature to obtain a composite layer coated glass, completing the surface coating process of the 3D automotive glass; The target material of the anti-fingerprint layer is a mixed target material. The preparation process of the mixed target material is as follows: titanium powder and polytetrafluoroethylene powder are fully stirred and mixed in a mass ratio of 1.25-1.3:1, and then pressed into blocks to obtain the mixed target material; The coating thickness of the anti-fingerprint layer is 45nm-150nm.

2. A 3D vehicle glass surface coating process according to claim 1, characterized in that: The protective gas is argon or nitrogen.

3. A 3D vehicle glass surface coating process according to claim 1, characterized in that: The target material of the high refractive index layer is one of TiO2, Nb2O5 and ZrO, and the coating thickness of the high refractive index layer is 30nm-75nm.

4. The 3D vehicle glass surface coating process according to claim 1, characterized in that: The target material of the low refractive index layer is one of SiO2 and AlF3, and the coating thickness of the low refractive index layer is 35nm-90nm.

5. The 3D vehicle glass surface coating process according to claim 1, characterized in that: The 3D automotive glass needs to be pretreated before coating: the coated base surface of the 3D automotive glass is ultrasonically cleaned for 15 minutes using anhydrous ethanol, then ultrasonically cleaned for 15 minutes using deionized water, and then placed in a drying room at 80° C. for 30 minutes to complete the pretreatment of the 3D automotive glass.