A kind of long afterglow microcrystalline glass and its preparation method and application
By using specific compositions and high-temperature heat treatment technology in long afterglow materials, the problems of poor water resistance and afterglow properties of existing materials are affected by matrix materials, and long afterglow microcrystalline glass with long afterglow time and high stability are prepared. In various light source excitation and wide application fields.
Patent Information
- Application Number
- CN202310094289.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-02-10
AI Technical Summary
The existing long afterglow materials excitated by solar light have poor water resistance, and their remaining light properties are easily restricted when used in matrix materials, which cannot effectively solve the problem of excitation light source and insufficient stability.
A preparation method is adopted, including mixing, melting, molding, annealing, nucleating and crystallizing the composition to obtain a long afterglow microcrystalline glass, which contains a specific molar ratio of SrO, MgO, SiO2, Al2O3, B2O3, Na2O, ZrO2, Eu2O3 and Dy2O3 improve the stability and optical properties of the material through high-temperature heat treatment.
The prepared long afterglow microcrystalline glass has a blue afterglow time of up to 26 hours, good thermal stability and physical and chemical stability, and strong weather resistance. It is suitable for night lighting, energy-saving indication and anti-counterfeiting fields, and is simple and costly. Low.
Smart Images

Figure CN116119930B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of microcrystalline glass, and in particular to a long afterglow microcrystalline glass and a preparation method and application thereof. Background Art
[0002] Long afterglow luminescent material is a material that can continue to emit light after the external excitation light source is removed. It has broad application prospects in night lighting, energy-saving indication, anti-counterfeiting and other fields.
[0003] Many traditional long afterglow materials require the stimulation of light sources such as ultraviolet light and X-rays to produce afterglow luminescence, which cannot be effectively used in some places where electricity is scarce. Long afterglow materials excited by sunlight can convert the absorbed solar energy into afterglow luminescence, which can well solve the problem of exciting light sources.
[0004] Most of the materials reported so far that can be excited by sunlight to produce long afterglow are phosphors. For example, SrAl2O4:Eu, Dy and Sr4Al 14 O 25 : Eu, Dy phosphors can be excited by sunlight to produce green afterglow, but their water resistance is poor and they can easily react with water to destroy their structure and weaken their afterglow performance.
[0005] Qi Xiaoxia used a high-temperature solid phase method to prepare Sr2MgSi2O7:Eu with high brightness and long afterglow time under carbon powder reduction conditions. 2+ ,Dy 3+ Long afterglow luminescent materials are prepared, and their performance and factors affecting their luminescent performance are studied. The emission spectrum of the luminescent powder after reduction shows that its main emission peak is located at around 463nm; the afterglow decay curve proves that there are two processes of afterglow decay, namely fast decay and slow decay. However, when the powder material prepared by the prior art is added to other matrix materials such as ink, the matrix material will restrict the afterglow performance of the powder additive.
[0006] Therefore, developing a long afterglow material that can be effectively excited by sunlight and has high stability has important scientific and applied research value. Summary of the invention
[0007] The purpose of the present invention is to provide a long afterglow glass-ceramic with a long afterglow time.
[0008] In order to achieve the above object, the first aspect of the present invention provides a method for preparing long afterglow glass-ceramics, the method comprising:
[0009] (1) mixing the components of a composition for preparing long afterglow glass-ceramics to obtain a mixture, and then subjecting the mixture to a melting treatment, a molding treatment, and an annealing treatment in sequence to obtain a base glass; the melting treatment is performed in the presence of carbon powder, and the weight ratio of the mixture to the carbon powder is 1:0.02-0.06;
[0010] (2) subjecting the base glass to a nucleation treatment and a crystallization treatment in sequence to obtain the long afterglow glass-ceramics; the conditions for the nucleation treatment include: a temperature of 600-700° C. and a time of 2-3 h; the conditions for the crystallization treatment include: a temperature of 800-1000° C. and a time of 1-2 h;
[0011] Based on the total molar amount of the composition, the composition contains 14.5-18.5 mol% SrO, 13.5-15.5 mol% MgO, 55-65 mol% SiO2, 3-5.5 mol% Al2O3, 0.5-1 mol% B2O3, 0.5-1.5 mol% Na2O, 0-2 mol% ZrO2, 0.05-0.1 mol% Eu2O3, and 0.05-0.1 mol% Dy2O3.
[0012] Preferably, based on the total molar amount of the composition, the composition contains 15-17 mol% SrO, 14-15 mol% MgO, 60-62 mol% SiO2, 3-4 mol% Al2O3, 0.5-1 mol% B2O3, 0.5-1 mol% Na2O, 1-1.5 mol% ZrO2, 0.05-0.1 mol% Eu2O3, and 0.05-0.1 mol% Dy2O3.
[0013] Preferably, in step (1), the weight ratio of the mixture to the carbon powder is 1:0.04-0.06.
[0014] Preferably, in step (1), the conditions of the melt treatment include: a temperature of 1450-1550° C. and a time of 3-4 hours.
[0015] Preferably, in step (1), the annealing treatment conditions include: a temperature of 500-600° C. and a time of 4-6 hours.
[0016] According to a preferred embodiment, in step (2), the heating rate of the nucleation treatment is 5-10°C / min.
[0017] According to another preferred embodiment, in step (2), the heating rate of the crystallization treatment is 3-5°C / min.
[0018] The second aspect of the present invention provides long afterglow glass-ceramics prepared by the method described in the first aspect.
[0019] Preferably, the main crystalline phase in the long afterglow glass-ceramics is Sr2MgSi2O7.
[0020] The third aspect of the present invention provides the use of the long afterglow glass-ceramics described in the second aspect in the field of energy-saving indication and / or anti-counterfeiting.
[0021] The long afterglow glass-ceramics provided by the present invention is a composite material in which micron crystals or nanocrystals are uniformly embedded in an inorganic glass matrix. It combines the advantages of crystals and materials, has optical properties similar to or better than those of crystals, and has a preparation method similar to that of glass materials and is simple to operate. The long afterglow glass-ceramics provided by the present invention has a long afterglow time, good thermal stability and physical and chemical stability, good weather resistance, and a long service life.
[0022] Compared with the prior art, the technical solution provided by the present invention also has the following advantages:
[0023] (1) In the present invention, Eu 2+ As an electron capture center and luminescence center, Dy 3+ It is a hole capture center that can effectively absorb sunlight, and after the light stops, the long afterglow micro-ceramic glass provided by the present invention can emit blue afterglow light for up to 26 hours;
[0024] (2) The present invention preferably uses high temperature heat treatment to controllably precipitate crystals in the glass, and the glass matrix can well cover the crystals, thereby improving the stability of the material;
[0025] (3) The preparation method provided by the present invention is simple, low-cost, and high-yield. It can be excited by a variety of external light sources and has a long afterglow time. It has broad application prospects in the fields of night lighting, energy-saving indication, anti-counterfeiting, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a process roadmap for preparing the long afterglow glass-ceramics of the present invention. DETAILED DESCRIPTION
[0027] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0028] As mentioned above, the first aspect of the present invention provides a method for preparing long afterglow glass-ceramics, the method comprising:
[0029] (1) mixing the components of the composition for preparing long afterglow glass-ceramics to obtain a mixture, and then subjecting the mixture to a melting treatment, a molding treatment, and an annealing treatment in sequence to obtain a base glass; the melting treatment is performed in the presence of carbon powder, and the weight ratio of the mixture to the carbon powder is 1:0.02-0.06;
[0030] (2) subjecting the base glass to a nucleation treatment and a crystallization treatment in sequence to obtain the long afterglow glass-ceramics; the conditions for the nucleation treatment include: a temperature of 600-700° C. and a time of 2-3 h; the conditions for the crystallization treatment include: a temperature of 800-1000° C. and a time of 1-2 h;
[0031] Based on the total molar weight of the composition, the composition contains 14.5-18.5 mol% SrO, 13.5-15.5 mol% MgO, 55-65 mol% SiO2, 3-5.5 mol% Al2O3, 0.5-1 mol% B2O3, 0.5-1.5 mol% Na2O, 0-2 mol% ZrO2, 0.5-1 mol% Eu2O3, and 0.5-1 mol% Dy2O3.
[0032] Preferably, based on the total molar amount of the composition, the composition contains 15-17 mol% SrO, 14-15 mol% MgO, 60-62 mol% SiO2, 3-4 mol% Al2O3, 0.5-1 mol% B2O3, 0.5-1 mol% Na2O, 1-1.5 mol% ZrO2, 0.5-1 mol% Eu2O3, and 0.5-1 mol% Dy2O3. The inventors of the present invention have found that under this preferred condition, the long afterglow glass-ceramics of the present invention has a more lasting afterglow time and better stability.
[0033] Preferably, the molar ratio of Eu2O3 to Dy2O3 in the composition is 1:0.5-2; the inventors of the present invention have found in their research that under this more preferred condition, the long afterglow microcrystalline glass of the present invention has a more lasting afterglow time and better stability.
[0034] The present invention has no particular limitation on the specific method of mixing in step (1), as long as the purpose of uniform mixing can be achieved. Those skilled in the art can select the method according to the technical means known in the art. For example, the components in the composition are placed in a mortar and ground for 30-60 minutes to make them uniformly mixed. The present invention will not be described in detail here, and those skilled in the art should not be construed as limiting the present invention.
[0035] Preferably, in step (1), the weight ratio of the mixture to the carbon powder is 1:0.04-0.06. The inventors of the present invention have found that under this preferred condition, the long afterglow glass-ceramics of the present invention has a more persistent afterglow time and better stability.
[0036] Preferably, in step (1), the conditions of the melt treatment include: a temperature of 1450-1550° C. and a time of 3-4 hours.
[0037] The present invention has no particular limitation on the molding process, and those skilled in the art can make a selection based on technical means known in the art. For example, the molten glass obtained after melting treatment is poured into a mold, and then cooled and molded to obtain block glass.
[0038] Preferably, in step (1), the annealing treatment conditions include: a temperature of 500-600° C. and a time of 4-6 hours.
[0039] Preferably, in step (1), the annealing treatment operation includes: placing the block glass obtained after forming into an annealing furnace with a set annealing temperature, and keeping the block glass warm for 4-6 hours after the annealing temperature reaches 500-600°C.
[0040] According to a preferred embodiment, in step (2), the heating rate of the nucleation treatment is 5-10°C / min.
[0041] According to another preferred embodiment, in step (2), the heating rate of the crystallization treatment is 3-5°C / min.
[0042] Figure 1 It shows a particularly preferred specific embodiment of the present invention, wherein the method for preparing long afterglow glass-ceramics comprises:
[0043] S1, ingredients: put each component of the composition for preparing long afterglow glass-ceramics in a mortar, grind for 30-60 minutes, and obtain a mixture;
[0044] S2, melting: in the presence of carbon powder, the mixture is melted at 1450-1550° C. for 3-4 hours to obtain glass liquid; the weight ratio of the mixture to the carbon powder is 1:0.02-0.06;
[0045] S3, molding and annealing: pouring the glass liquid into a mold, cooling and molding to obtain block glass, and annealing the block glass at 500-600° C. for 4-6 hours to obtain basic glass;
[0046] S4, nucleation: heating the base glass to 600-700° C. at a heating rate of 5-10° C. / min and keeping the temperature for 2-3 hours to perform nucleation treatment to obtain an intermediate product;
[0047] S5, crystallization: then the intermediate product is heated to 800-1000°C at a heating rate of 3-5°C / min and kept at that temperature for 1-2h for crystallization treatment to obtain the long afterglow glass-ceramics.
[0048] The method of the present invention may also include various conventional post-processing methods in the art, for example, the product obtained after the crystallization process may be cut and polished to obtain the long afterglow glass-ceramics. The present invention will not be described in detail here, and those skilled in the art should not be construed as limiting the present invention.
[0049] As mentioned above, the second aspect of the present invention provides a long afterglow glass-ceramics prepared by the method described in the first aspect.
[0050] Preferably, the main crystalline phase in the long afterglow glass-ceramics is Sr2MgSi2O7. The inventors of the present invention have found that under this preferred condition, the long afterglow glass-ceramics of the present invention has a more persistent afterglow time and better stability.
[0051] As mentioned above, the third aspect of the present invention provides the use of the long afterglow glass-ceramics described in the second aspect in the field of energy-saving indication and / or anti-counterfeiting.
[0052] In the present invention, Eu 2+ Can partially replace Sr 2+ Enter the middle of the lattice and can act as an electron capture center, Dy 3+ When excited by sunlight, ultraviolet light or fluorescent light, Eu 2+ Captured electrons become Eu + The generated holes are transported to Dy 3+ Dy 4+After the excitation stops, the holes escape due to thermal motion, and the afterglow luminescence of Eu is triggered by the reverse process. This material has broad application prospects in the fields of night lighting, energy-saving indication, anti-counterfeiting, etc.
[0053] The present invention will be described in detail below by way of examples. Unless otherwise specified, the raw materials used in the following examples are all commercially available products.
[0054] Unless otherwise specified, the amounts of components in the formulations involved in the following examples are expressed in molar percentage. Taking the molar percentage of SiO2 in Example 1 as an example, the calculation method is: molar percentage of SiO2 = (molar amount of SiO2) / (the sum of the molar amounts of each component in Example 1) × 100%.
[0055] Unless otherwise specified, in the following examples, the sum of the molar amounts of the components in the composition for preparing long afterglow glass-ceramics is determined to be 100 mol for testing, and the masses of the corresponding components are calculated based on the formula of the glass composition and accurately weighed (to two decimal places).
[0056] Example 1
[0057] S1: According to the formula shown in Table 1, each component in the composition for preparing long afterglow glass-ceramics is placed in a mortar and ground for 30 minutes to obtain a mixture;
[0058] S2: pour the mixture into an alumina crucible, then put the crucible containing the mixture into a large crucible containing carbon powder (the weight ratio of the mixture to the carbon powder is 1:0.04), and then melt the mixture at 1500°C for 4 hours to obtain glass liquid;
[0059] S3: pouring the glass liquid into a mold, cooling and molding it to obtain a block of glass, and quickly transferring it to a muffle furnace, keeping it at 550° C. for 6 hours for annealing treatment to obtain a base glass;
[0060] S4: heating the base glass to 650°C at a heating rate of 10°C / min and keeping the temperature for 3 hours to perform a nucleation treatment to obtain an intermediate product;
[0061] S5: Then, the intermediate product is heated to 950°C at a heating rate of 3°C / min and kept at this temperature for 2 hours for crystallization treatment to obtain a microcrystalline glass sample.
[0062] Example 2
[0063] S1: According to the formula shown in Table 1, each component in the composition for preparing long afterglow glass-ceramics is placed in a mortar and ground for 40 minutes to obtain a mixture;
[0064] S2: pour the mixture into an alumina crucible, then put the crucible containing the mixture into a large crucible containing carbon powder (the weight ratio of the mixture to the carbon powder is 1:0.05), and then melt the mixture at 1450°C for 3 hours to obtain glass liquid;
[0065] S3: pouring the glass liquid into a mold, cooling and molding it to obtain a block of glass, and quickly transferring it to a muffle furnace, keeping it at 500°C for 4 hours for annealing treatment to obtain a base glass;
[0066] S4: heating the base glass to 600°C at a heating rate of 5°C / min and keeping the temperature for 3 hours to perform a nucleation treatment to obtain an intermediate product;
[0067] S5: Then, the intermediate product is heated to 800°C at a heating rate of 3°C / min and kept at that temperature for 1 hour for crystallization treatment to obtain a microcrystalline glass sample.
[0068] Example 3
[0069] S1: According to the formula shown in Table 1, each component in the composition for preparing long afterglow glass-ceramics is placed in a mortar and ground for 30 minutes to obtain a mixture;
[0070] S2: pour the mixture into an alumina crucible, then put the crucible containing the mixture into a large crucible containing carbon powder (the weight ratio of the mixture to the carbon powder is 1:0.06), and then melt the mixture at 1550°C for 4 hours to obtain glass liquid;
[0071] S3: pouring the glass liquid into a mold, cooling and molding it to obtain a block of glass, and quickly transferring it to a muffle furnace, keeping it at 600°C for 6 hours for annealing treatment, and obtaining a base glass;
[0072] S4: heating the base glass to 700°C at a heating rate of 10°C / min and keeping the temperature for 3 hours to perform a nucleation treatment to obtain an intermediate product;
[0073] S5: Then, the intermediate product is heated to 1000°C at a heating rate of 5°C / min and kept at that temperature for 2 hours for crystallization treatment to obtain a microcrystalline glass sample.
[0074] Example 4
[0075] This embodiment adopts a process similar to that of Embodiment 1, except that in step S2, the composition and amount of the mixture remain unchanged, and the weight ratio of the mixture to the carbon powder is adjusted to 1:0.02.
[0076] A glass-ceramic sample was prepared.
[0077] The microcrystalline glass samples of Comparative Examples 1, 2 and 3 are all prepared using a process similar to that of Example 1, except that the total molar amount of each component used to prepare the long afterglow microcrystalline glass remains unchanged, and the amount of each component in the composition is adjusted, as shown in Table 1.
[0078] Comparative Example 4
[0079] This comparative example is carried out using a process similar to that of Example 1, except that in step S2, the composition and amount of the mixture remain unchanged, and the weight ratio of the mixture to the carbon powder is adjusted to 1:0.01.
[0080] A glass-ceramic sample was prepared.
[0081] Test Case
[0082] The main crystalline phase of the microcrystalline glass in the above-mentioned embodiments and comparative examples was determined by X-ray powder diffraction analysis. The X-ray powder diffractometer model used was D8 Advance, which was purchased from Bruker of Germany. The testing method was as follows: the microcrystalline glass to be tested was crushed and ground, and an appropriate amount of the ground powder was placed in an X-ray diffractometer to test its diffraction pattern, and the main crystalline phase of the microcrystalline glass was determined based on its diffraction pattern.
[0083] Afterglow time test method: The microcrystalline glass prepared in the aforementioned embodiments and comparative examples was irradiated by a 365nm ultraviolet light source for more than 10 minutes, or irradiated in the sun for more than 15 minutes. After stopping the irradiation, the afterglow of the microcrystalline glass was observed. The results are shown in Table 1.
[0084] Table 1
[0085] Component (mol%) Example 1 Example 2 Example 3 Example 4 SrO 15 17 16 15 MgO 14 15 15 14 <![CDATA[SiO2]]> 63 60 61 63 <![CDATA[Al2O3]]> 4 3 4 4 <![CDATA[B2O3]]> 1 1 0.5 1 <![CDATA[Na2O]]> 1 1 0.5 1 <![CDATA[ZrO2]]> 1 1.5 1.5 1 <![CDATA[Eu2O3]]> 0.5 0.5 1 0.5 <![CDATA[Dy2O3]]> 0.5 1 0.5 0.5 Main crystal phase <![CDATA[Sr2MgSi2O7]]> <![CDATA[Sr2MgSi2O7]]> <![CDATA[Sr2MgSi2O7]]> <![CDATA[Sr2MgSi2O7]]> Persistence Color blue blue blue blue Afterglow time (h) 26 26 26 22
[0086] Table 1
[0087] Component (mol%) Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 SrO 15 15 19 15 MgO 14 14 16 14 <![CDATA[SiO2]]> 63 62 57.4 63 <![CDATA[Al2O3]]> 4 4 4 4 <![CDATA[B2O3]]> 1 1 1 1 <![CDATA[Na2O]]> 1 1 1 1 <![CDATA[ZrO2]]> 1 1 1 1 <![CDATA[Eu2O3]]> 0 1 0.3 0.5 <![CDATA[Dy2O3]]> 1 0 0.3 0.5 Main crystal phase <![CDATA[Sr2MgSi2O7]]> <![CDATA[Sr2MgSi2O7]]> <![CDATA[Sr2MgSi2O7]]> <![CDATA[Sr2MgSi2O7]]> Persistence Color none blue blue blue Afterglow time (h) 0 5 12 10
[0088] It can be seen from the above results that the afterglow time of the long afterglow microcrystalline glass prepared by the technical solution provided by the present invention is significantly better than that of the comparative example, and has broad application prospects in the fields of night lighting, energy-saving indication, anti-counterfeiting, etc.
[0089] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing long afterglow glass-ceramics, characterized in that: The method includes: (1) mixing the components of the composition for preparing long afterglow glass-ceramics to obtain a mixture, and then subjecting the mixture to a melting treatment, a molding treatment, and an annealing treatment in sequence to obtain a base glass; the melting treatment is performed in the presence of carbon powder, and the weight ratio of the mixture to the carbon powder is 1:0.02-0.06; (2) subjecting the base glass to a nucleation treatment and a crystallization treatment in sequence to obtain the long afterglow glass-ceramics; the conditions for the nucleation treatment include: a temperature of 600-700° C. and a time of 2-3 h; the conditions for the crystallization treatment include: a temperature of 800-1000° C. and a time of 1-2 h; the main crystalline phase in the long afterglow glass-ceramics is Sr2MgSi2O7; Based on the total molar amount of the composition, the composition contains 15-17 mol% SrO, 14-15 mol% MgO, 60-63 mol% SiO2, 3-4 mol% Al2O3, 0.5-1 mol% B2O3, 0.5-1 mol% Na2O, 1-1.5 mol% ZrO2, 0.5-1 mol% Eu2O3, and 0.5-1 mol% Dy2O3.
2. The method according to claim 1, characterized in that Based on the total molar amount of the composition, the composition contains 15-17 mol% SrO, 14-15 mol% MgO, 60-62 mol% SiO2, 3-4 mol% Al2O3, 0.5-1 mol% B2O3, 0.5-1 mol% Na2O, 1-1.5 mol% ZrO2, 0.5-1 mol% Eu2O3, and 0.5-1 mol% Dy2O3.
3. The method according to claim 1 or 2, characterized in that: In step (1), the weight ratio of the mixture to the carbon powder is 1:0.04-0.
06.
4. The method according to claim 1 or 2, characterized in that: In step (1), the conditions of the melt treatment include: a temperature of 1450-1550° C. and a time of 3-4 hours.
5. The method according to claim 1 or 2, characterized in that: In step (1), the annealing treatment conditions include: temperature of 500-600° C. and time of 4-6 hours.
6. The method according to claim 1 or 2, characterized in that: In step (2), the heating rate of the nucleation treatment is 5-10°C / min.
7. The method according to claim 1 or 2, characterized in that: In step (2), the heating rate of the crystallization treatment is 3-5°C / min.
8. Long afterglow glass-ceramics prepared by the method described in any one of claims 1 to 7; the main crystalline phase in the long afterglow glass-ceramics is Sr2MgSi2O7.
9. Application of the long afterglow glass-ceramics described in claim 8 in the field of energy-saving indication and / or anti-counterfeiting.
Citation Information
Patent Citations
Red long-afterglow phosphor and preparation method thereof
CN107746708A
Blue long-afterglow fluorescent powder and preparation method thereof
CN107828412A
Long-afterglow light-emitting microcrystal glass and preparation method thereof
CN108059352A
Preparation method of yellow-green long-afterglow fluorescent material and application of ammonium bicarbonate
CN111635757A
Red-light-emitting glass ceramic and preparation method thereof, and LED / LD light emitting device
CN112194376A