A kind of anti-ultraviolet coating and preparation method thereof

By using stearic acid and polyvinylpyrrolidone modified nanotitanium dioxide, combined with self-emulsified epoxy resin and epoxy resin modified silicon acrylic emulsion, the dispersion and stability of nanotitanium dioxide in the coating are solved, and high UV resistance is achieved and low-cost coating preparation improve the overall performance of the coating.

CN116120806BActive Publication Date: 2024-11-15GUANGDONG TUBAINIAN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211705755.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-11-15
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

Existing UV-proof coatings have challenges between improving UV-proof effects and reducing production costs, and the dispersion and stability of nanotitanium dioxide in coatings are difficult to solve, resulting in limited UV-proof performance.

Method used

采用硬脂酸和聚乙烯吡咯烷酮改性的纳米二氧化钛,并通过控制分散剂配比和二氧化钛的平均粒径,结合自乳化环氧树脂乳液和环氧树脂改性硅丙乳液,制备出具有高防紫外线性能的涂料,提高涂料的耐紫外线、耐水性和耐擦洗性能。

Benefits of technology

It achieves high storage stability, hardness and excellent UV resistance of the paint, reduces production costs, and improves the acid and alkali resistance and scrubbing resistance of the paint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004026320270000071
    Figure BDA0004026320270000071
Patent Text Reader

Abstract

The present invention relates to a kind of anti-ultraviolet coating and preparation method thereof, and the raw materials for preparing the coating include: 40-50 parts of self-emulsifying epoxy resin emulsion, 10-15 parts of epoxy resin modified silicone acrylic emulsion, 15-25 parts of alkyd resin, 25-55 parts of nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone, 5-9 parts of dispersant, 0.5-2 parts of defoamer, 1-3 parts of wetting agent, 0.2-0.4 parts of dioctyl phthalate, 100-200 parts of water; the water does not include the water contained in the modified nano titanium dioxide; the dispersant includes a combination of sodium oleate and polyethylene glycol. The coating of the present invention has good storage stability, and the hardness of the paint film is high, which is conducive to resisting physical damage; it has excellent water resistance, acid and alkali resistance and scrub resistance; and it has excellent anti-ultraviolet performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chemical industry, and more particularly to an anti-ultraviolet coating and a preparation method thereof. Background Art

[0002] Light, heat, water, oxygen, inorganic salts, organic solvents and pollutants in the environment are the main factors that cause the degradation of film-forming substances. Among these factors, sunlight ultraviolet radiation is the most important and common factor that causes the degradation of film-forming substances. From the moment the exterior wall paint is used, its irreversible degradation process begins. Therefore, it is necessary to enhance the anti-ultraviolet performance of exterior wall paint. The simplest and most effective method is to add additives with anti-ultraviolet performance to the exterior wall paint, mainly organic ultraviolet shielding agents and inorganic ultraviolet shielding agents.

[0003] Anti-ultraviolet paint, as the name implies, is a paint that can effectively resist aging due to ultraviolet radiation. In the United States, Foster Products uses nano-grade zinc oxide, hydroxyethyl cellulose as a thickener, and other additives to fully disperse with water, and then stir and mix with acrylic emulsion to produce water-based paint that resists ultraviolet aging. In addition, Elementis, an American company, uses nano-ZnO with a particle size of about 80nm produced by the company, and compounds it with certain solvents, resins, additives and organic anti-ultraviolet agents to produce anti-ultraviolet premixes, which can be used as part of coating and plastic formulas.

[0004] Currently, the widely used organic UV shielding agents include o-hydroxybenzophenone, o-hydroxybenzotriazole, o-hydroxyphenyltriazine, salicylate, benzoate, cinnamate and oxalic acid anilide, but there are many disadvantages in adding organic UV shielding agents to improve the UV protection performance of coatings. First, organic UV shielding agents have certain toxicity; second, organic UV shielding agents have selective absorption of ultraviolet rays; finally, over time, the UV protection performance of organic UV shielding agents will gradually weaken or even disappear.

[0005] Inorganic UV shielding agents mainly include nano titanium dioxide, nano silicon dioxide and nano zinc oxide. Nano titanium dioxide has attracted much attention due to its stable chemical properties, non-toxicity, low price and strong UV shielding performance. Nano titanium dioxide has strong UV shielding performance, and the smaller the particle size, the stronger the UV shielding performance. Submicron titanium dioxide hardly shields UV rays. The UV shielding performance of nano titanium dioxide is determined by its absorption and scattering abilities. The absorption of ultraviolet rays by nano titanium dioxide is mainly due to its semiconductor properties. Under ultraviolet irradiation, the electrons are excited and transition from the valence band to the conduction band, causing the absorption of ultraviolet rays. Nano titanium dioxide not only has the ability to absorb ultraviolet rays, but also has the ability to scatter ultraviolet rays. Ultraviolet rays are essentially an electromagnetic wave. When ultraviolet rays act on nano titanium dioxide in the medium, since the size of nano titanium dioxide particles is smaller than the wavelength of ultraviolet rays, the electrons in the nano titanium dioxide particles are forced to vibrate (their vibration frequency is the same as the frequency of the incident light wave), becoming a secondary wave source, emitting electromagnetic waves in all directions. This is the scattering of ultraviolet rays.

[0006] However, the dispersibility and stability of nano titanium dioxide in the coating are the key problems to be solved by the nano coating. In view of this problem, China's authorized patent CN105017871B discloses an anti-ultraviolet exterior wall coating and its preparation method, wherein the preparation method first coats a layer of acrylate polymer on the surface of nano titanium dioxide to obtain a nano titanium dioxide / acrylate polymer composite emulsion, then fully mixes the composite emulsion with the acrylate polymer exterior wall emulsion, and then adds pigments, fillers, additives and water. The coating coats a layer of acrylate polymer on the surface of nano titanium dioxide, significantly improving the dispersibility and stability of nano titanium dioxide in the coating, avoiding the formation of nano titanium dioxide agglomerates, and the anti-ultraviolet performance of the agglomerates will be greatly reduced or even absent. The coating not only has the excellent water resistance, alkali resistance and scrub resistance of acrylate polymer exterior wall coatings, but also improves its hardness and anti-ultraviolet performance, and prolongs the service life of the coating. However, the coating involves coating a layer of acrylate polymer on the surface of nano titanium dioxide to obtain a nano titanium dioxide / acrylate polymer composite emulsion, and its preparation process is relatively complicated and the production cost is relatively high.

[0007] In addition, China's authorized patent CN104403428B discloses an anti-ultraviolet coating that does not contain toxic ultraviolet absorbers and a preparation method thereof. The coating is composed of the following raw materials, and the parts are all in weight: 30-40 parts of polystyrene latex; 10-16 parts of epoxy resin primer; 2-8 parts of leveling agent; 17-20 parts of ultraviolet absorber; 10-18 parts of inorganic filler; wherein the ultraviolet absorber is composed of the following parts of components, and the parts are all in weight: 14-15 parts of 2-hydroxy-4-n-octyloxybenzophenone; 3-5 parts of phenyl o-hydroxybenzoate. The anti-ultraviolet coating disclosed in the invention does not contain toxic ultraviolet absorbers, is safe and harmless to humans and the environment, and is beneficial to environmental protection and construction safety; the added epoxy resin primer can increase the adhesion of the coating on the surface of the object; the polystyrene latex is synthesized by the microemulsion method, and the synthesized polystyrene latex has the advantages of small particle size, good dispersibility, good stability, etc., which is beneficial to the coating; the addition of inorganic fillers can increase the hardness, strength and wear resistance of the coating; the preparation process of the anti-ultraviolet coating of the invention is simple and easy to operate.

[0008] In the prior application CN115074000A of the present applicant, an anti-ultraviolet coating and its preparation method are also disclosed, and the raw materials for preparing the coating include: 40-50 parts of self-emulsifying epoxy resin emulsion, 10-15 parts of epoxy resin modified silicone acrylic emulsion, 15-25 parts of alkyd resin, 25-55 parts of nano titanium dioxide modified by sodium alginate, 5-9 parts of dispersant, 0.5-2 parts of defoamer, 1-3 parts of wetting agent, 0.2-0.4 parts of dioctyl phthalate, and 100-200 parts of water; the water does not include the water contained in the nano titanium dioxide modified by sodium alginate; the dispersant includes a combination of sodium oleate and polyethylene glycol. However, the anti-ultraviolet ability of the anti-ultraviolet coating disclosed in the prior application is still limited, and there is room for further improvement.

[0009] Although there are anti-ultraviolet coatings, how to further reduce the production cost and obtain coatings with good stability and anti-ultraviolet effect is still a technical problem to be solved by those skilled in the art. This application is based on the applicant's prior application CN115074000A and is completed through further creative research. Summary of the invention

[0010] Based on the above background technology, the technical problem to be solved by the present invention is to provide a coating with reduced production cost and good stability and UV protection effect. In order to achieve the purpose of the present invention, the following technical scheme is proposed:

[0011] One aspect of the present invention relates to an anti-ultraviolet coating, characterized in that the raw materials for preparing the coating include:

[0012] 40-50 parts of self-emulsifying epoxy resin emulsion, 10-15 parts of epoxy resin modified silicone acrylic emulsion, 15-25 parts of alkyd resin, 25-55 parts of nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone, 5-9 parts of dispersant, 0.5-2 parts of defoamer, 1-3 parts of wetting agent, 0.2-0.4 parts of dioctyl phthalate, and 100-200 parts of water; the water does not include the water contained in the nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone;

[0013] The dispersant includes a combination of sodium oleate and polyethylene glycol;

[0014] The stearic acid and polyvinyl pyrrolidone modified nano titanium dioxide is prepared by the following method:

[0015] Dissolve 0.5-1 parts by weight of stearic acid and 1-2 parts by weight of polyvinyl pyrrolidone in 50-100 parts of water, add 3-8 parts by weight of titanium dioxide with an average particle size of 50-150 nm, stir evenly and let stand to form nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone.

[0016] In a preferred embodiment of the present invention, the dispersant is prepared by mixing sodium oleate and polyethylene glycol in a mass ratio of 1-2:1-2. The present invention helps to improve the UV resistance of the coating by controlling the ratio of the dispersant.

[0017] In a preferred embodiment of the present invention, the weight ratio of stearic acid to polyvinyl pyrrolidone is 1: 4. By adopting this preferred weight ratio, the UV protection capability of the coating can be further improved.

[0018] In a preferred embodiment of the present invention, the average particle size of the titanium dioxide is 50-75 nm. By controlling the average particle size of the titanium dioxide within this preferred range, it is helpful to improve the UV resistance of the coating.

[0019] In a preferred embodiment of the present invention, the average particle size of the titanium dioxide is 90-110 nm. By controlling the average particle size of the titanium dioxide within this preferred range, it is helpful to improve the scrub resistance of the coating.

[0020] Another aspect of the present invention also relates to a method for preparing the above-mentioned coating, which is characterized by comprising the following steps:

[0021] Put water, self-emulsifying epoxy resin emulsion, epoxy resin modified silicone acrylic emulsion and alkyd resin into the mixing kettle in turn, stir and mix at a speed of 200-400rpm for 10-20min; increase the speed to 450-700rpm, add nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone, stir for 3-8min and then heat to 40-50℃; take samples for testing and when the fineness is ≤25μm, add dispersant, defoamer, wetting agent and dioctyl phthalate, increase the speed to 800-1200rpm and stir; take samples from the mixing kettle every 8-12min, apply and scrape on the glass plate to see if there is no shrinkage cavity, cool to room temperature and package.

[0022] In a preferred embodiment of the present invention, the preparation method of the self-emulsifying epoxy resin emulsion is as follows:

[0023] Sodium dodecylbenzene sulfonate, polyoxyethylene sorbitan monooleate, bisphenol A epoxy resin and bisphenol A are added into the reactor, heated to 130-150°C with stirring for 20-40 minutes, triphenylphosphine is slowly added, and the system is monitored at any time. When the epoxy value of the system is less than 0.2, the reaction system is cooled to 60-80°C, propylene glycol butyl ether and benzyl alcohol are added, and stirring is continued for 30-50 minutes. Water is added and stirring is continued at high speed for 5-10 minutes.

[0024] In a preferred embodiment of the present invention, the preparation method of the epoxy resin modified silicone acrylic emulsion is as follows:

[0025] Add sodium dodecylbenzene sulfonate and acrylic acid monomer into water, heat to 70-75°C and stir for 10-15 minutes, slowly drop 1-5% sodium persulfate solution, continue stirring for 30-50 minutes, then add epoxy resin and silicone emulsion, heat to 80-85°C and stir for 3-4 hours, then cool to 40-50°C, adjust the pH of the system to 8 with ammonia water, and filter.

[0026] Beneficial Effects

[0027] The coating of the present invention has good storage stability and high hardness of the paint film, which is conducive to resisting physical damage; it has excellent water resistance, acid and alkali resistance and scrub resistance; and its UV protection performance is further optimized. DETAILED DESCRIPTION

[0028] In order to further understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Unless otherwise specified, the reagents involved in the embodiments of the present invention are all commercially available products and can be purchased through commercial channels.

[0030] Embodiment 1:

[0031] An anti-ultraviolet coating, the coating contains the following components in parts by weight:

[0032] 44 parts of self-emulsifying epoxy resin emulsion, 12 parts of epoxy resin modified silicone acrylic emulsion, 20 parts of alkyd resin, 30 parts of nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone, 7 parts of dispersant obtained by compounding sodium oleate and polyethylene glycol in a mass ratio of 1:1, 1 part of defoamer BKY-020, 2 parts of wetting agent X405, 0.3 parts of dioctyl phthalate, and 150 parts of water.

[0033] Wherein, the preparation method of self-emulsifying epoxy resin emulsion is as follows:

[0034] Sodium dodecylbenzene sulfonate, polyoxyethylene sorbitan monooleate, bisphenol A epoxy resin and bisphenol A are added into the reactor. After stirring and heating to 140°C for 25 minutes, triphenylphosphine is slowly added and monitored at any time. When the epoxy value of the system is less than 0.2, the reaction system is cooled to 60°C, propylene glycol butyl ether and benzyl alcohol are added, and stirring is continued for 35 minutes. Water is added and stirring is continued at high speed for 5 minutes.

[0035] Wherein, the preparation method of epoxy resin modified silicone acrylic emulsion is as follows:

[0036] Add sodium dodecylbenzene sulfonate and acrylic acid monomer into water, heat to 70°C and stir for 12 minutes, slowly drop 2% sodium persulfate solution, continue stirring for 50 minutes, then add epoxy resin and silicone emulsion, heat to 80°C and stir for 4 hours, then cool to 40°C, adjust the pH of the system to 8 with ammonia water, and filter.

[0037] The preparation method of nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone is as follows:

[0038] 0.5 parts by weight of stearic acid and 1.4 parts by weight of polyvinyl pyrrolidone were dissolved in 50 parts of water, and 5 parts by weight of titanium dioxide with an average particle size of 55 nm was added. After stirring evenly, the mixture was allowed to stand to form nano titanium dioxide modified with stearic acid and polyvinyl pyrrolidone.

[0039] The present invention also provides a method for preparing the above ecological water-based paint as follows:

[0040] Put water, self-emulsifying epoxy resin emulsion, epoxy resin modified silicone acrylic emulsion and alkyd resin into the mixing kettle in turn, stir and mix at a speed of 300 rpm for 20 minutes; increase the speed to 600 rpm, add stearic acid and nano titanium dioxide modified by polyvinyl pyrrolidone, stir for 5 minutes and then heat to 45°C; take samples for testing and when the fineness is ≤25μm, add dispersant, defoamer BKY-020, wetting agent X405 and dioctyl phthalate, increase the speed to 1000 rpm and stir; take samples from the mixing kettle every 10 minutes, apply and scrape on the glass plate to see if there is no shrinkage cavity, cool to room temperature and package.

[0041] Embodiment 2:

[0042] The same as Example 1, except that 0.5 parts by weight of stearic acid and 2.0 parts by weight of polyvinyl pyrrolidone are used to modify the nano titanium dioxide.

[0043] Embodiment 3:

[0044] The same as Example 1, except that the average particle size of titanium dioxide is 100 nm.

[0045] Comparative Example 1:

[0046] The same as Example 1, except that 2.0 parts by weight of stearic acid is used instead of stearic acid and polyvinyl pyrrolidone.

[0047] Comparative Example 2:

[0048] The same as Example 1, except that 2.0 parts by weight of polyvinyl pyrrolidone is used instead of stearic acid and polyvinyl pyrrolidone.

[0049] Comparative Example 3:

[0050] The same as Example 1, except that nano zinc oxide with an average particle size of 65 nm is used instead of nano titanium dioxide.

[0051] Test Description

[0052] The anti-ultraviolet coatings prepared in Examples 1-3 and Comparative Examples 1-3 were tested:

[0053] The storage stability of the coating was tested at high temperature (50°C) for 2 months. No floating oil and no precipitation were recorded as ++, floating oil or precipitation were recorded as +, and both floating oil and precipitation were recorded as -.

[0054] The UV protection performance of the paint film was tested using an accelerated aging instrument. The UV light source was a UVA-340nm lamp with an irradiation intensity of 1.0W / m 2 , record the time when the coating film (thickness 1mm) formed by the coating begins to powder, bubble and / or crack;

[0055] Determine the hardness of the paint film according to GB / T6739-2006;

[0056] Determine the water resistance of the paint film according to GB5209-1985;

[0057] Determine the alkali resistance of the paint film according to GB9274-1988;

[0058] The scrub resistance of the paint film was determined according to GB / T9266-88.

[0059] Table 1 Test results of UV protection coating performance

[0060]

[0061] The above experimental results show that the coating of the present invention has good storage stability, and the hardness of the paint film is high, which is conducive to resisting physical damage; it has excellent water resistance, acid and alkali resistance and scrub resistance; and it has excellent UV resistance. In particular, the UV resistance of Example 2 is the best.

[0062] The above describes the preferred embodiments of the present invention, but it is not intended to limit the present invention. Those skilled in the art may make improvements and changes to the embodiments disclosed herein without departing from the scope and spirit of the present invention.

Claims

1. An anti-ultraviolet coating, characterized in that The raw materials for preparing the coating include: 40-50 parts of self-emulsifying epoxy resin emulsion, 10-15 parts of epoxy resin modified silicone acrylic emulsion, 15-25 parts of alkyd resin, 25-55 parts of nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone, 5-9 parts of dispersant, 0.5-2 parts of defoamer, 1-3 parts of wetting agent, 0.2-0.4 parts of dioctyl phthalate, and 100-200 parts of water; the water does not include the water contained in the nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone; The dispersant is composed of sodium oleate and polyethylene glycol in a mass ratio of 1-2:1-2; The stearic acid and polyvinyl pyrrolidone modified nano titanium dioxide is prepared by the following method: Dissolve 0.5-1 parts by weight of stearic acid and 1-2 parts by weight of polyvinyl pyrrolidone in 50-100 parts of water, add 3-8 parts by weight of titanium dioxide with an average particle size of 50-150 nm, stir evenly and let stand to form nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone; The weight ratio of stearic acid to polyvinyl pyrrolidone is 1:4; and the average particle size of titanium dioxide is 50-75nm or 90-110nm.

2. The method for preparing the coating according to claim 1, characterized in that The steps include: Put water, self-emulsifying epoxy resin emulsion, epoxy resin modified silicone acrylic emulsion and alkyd resin into the mixing kettle in turn, stir and mix at a speed of 200-400rpm for 10-20min; increase the speed to 450-700rpm, add nano titanium dioxide modified by stearic acid and polyvinyl pyrrolidone, stir for 3-8min and then heat to 40-50℃; take samples for testing and when the fineness is ≤25μm, add dispersant, defoamer, wetting agent and dioctyl phthalate, increase the speed to 800-1200rpm and stir; take samples from the mixing kettle every 8-12min, apply and scrape on the glass plate to see if there is no shrinkage cavity, cool to room temperature and package.

3. The preparation method according to claim 2, wherein the preparation method of the self-emulsifying epoxy resin emulsion is as follows: Sodium dodecylbenzene sulfonate, polyoxyethylene sorbitan monooleate, bisphenol A epoxy resin and bisphenol A are added into the reactor, heated to 130-150°C with stirring for 20-40 minutes, triphenylphosphine is slowly added, and the system is monitored at any time. When the epoxy value of the system is less than 0.2, the reaction system is cooled to 60-80°C, propylene glycol butyl ether and benzyl alcohol are added, and stirring is continued for 30-50 minutes. Water is added and stirring is continued at high speed for 5-10 minutes.

4. The preparation method according to claim 2, wherein the preparation method of the epoxy resin modified silicone acrylic emulsion is as follows: Add sodium dodecylbenzene sulfonate and acrylic acid monomer into water, heat to 70-75°C and stir for 10-15 minutes, slowly drop 1-5% sodium persulfate solution, continue stirring for 30-50 minutes, then add epoxy resin and silicone emulsion, heat to 80-85°C and stir for 3-4 hours, then cool to 40-50°C, adjust the pH of the system to 8 with ammonia water, and filter.