A100 ultra-high strength steel wire for additive manufacturing and cold working method thereof

Through rotary forging and drawing and bright annealing processes, the problem of difficult surface quality in traditional A100 ultra-high strength steel wire processing is solved, and high-precision and low-cost wire production is achieved, meeting the technical requirements of additive manufacturing.

CN116144898BActive Publication Date: 2024-11-05CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211105482.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-11-05
Estimated Expiration
2042-09-09

AI Technical Summary

Technical Problem

In the cold drawing process of traditional A100 ultra-high strength steel wire, the fixed mold pulling and intermediate heat treatment lead to large sliding friction between the wire and the mold surface, which is difficult to ensure the surface quality, and is prone to break during the processing, resulting in high processing difficulty and production efficiency. Low and high production costs.

Method used

Rotary forging drawing and bright annealing processes are adopted to replace the traditional fixed die wire drawing and annealing pickling processes. Through multiple rotary forging drawing and bright annealing, the number of deformations is reduced, production costs are reduced, secondary oxidation is avoided, and surface quality is improved.

Benefits of technology

It achieves high appearance and dimensional accuracy of silk material, smooth and defect-free surface, meets the technical requirements of additive manufacturing, reduces production costs, and avoids environmental pollution caused by pickling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116144898B_ABST
    Figure CN116144898B_ABST
Patent Text Reader

Abstract

The present invention provides an A100 ultra-high strength steel wire for additive manufacturing and a cold processing method thereof, wherein the A100 ultra-high strength steel wire is a material obtained by bright annealing, rotary forging drawing and tension straightening. The method of the present invention comprises the following steps: S1, using the A100 ultra-high strength steel hot-rolled coil as a raw material, removing the surface oxide layer; S2, placing the A100 ultra-high strength steel hot-rolled coil treated in step S1 in a hydrogen annealing furnace for bright annealing; S3, performing multiple passes of rotary forging drawing and bright annealing on the material obtained after the annealing treatment in step S2 to obtain a wire blank; S4, performing the last pass of rotary forging drawing on the wire blank obtained in step S3 to obtain a finished wire; S5, placing the finished wire obtained in step S4 in a hydrogen annealing furnace for bright annealing; S6, performing tension straightening on the wire obtained in step S5 to obtain an A100 ultra-high strength steel wire. The invention can stably produce the product with high dimensional accuracy, good surface quality and superior performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of wire preparation for additive manufacturing, and in particular to an A100 ultra-high strength steel wire for additive manufacturing and a cold processing method thereof. Background Art

[0002] A100 is a high-cobalt-nickel, secondary hardening type ultra-high strength steel. Due to its extremely high tensile strength and fracture toughness, it is mainly used in engine landing gear and various heavy-load bearing components. The traditional landing gear manufacturing process uses the forging + machining method, which has the problems of long manufacturing cycle, low material utilization rate and high production cost. With the rapid development of additive manufacturing technology, the use of additive manufacturing technology to produce landing gear can greatly reduce the production cycle, improve material utilization rate, and quickly respond to the development of new models. Therefore, it is necessary to develop A100 ultra-high strength steel wire for additive manufacturing.

[0003] The extremely high strength of A100 steel results in its poor processing performance. Traditional wire cold drawing adopts a production process of multi-pass fixed die drawing and intermediate heat treatment. During the processing, the sliding friction between the wire and the die surface is large, the surface quality is difficult to guarantee, and breakage is prone to occur during the processing. Therefore, the processing is difficult, the production efficiency is low, and the production cost is high. Summary of the invention

[0004] According to the above-mentioned traditional wire cold drawing production process using multiple fixed die drawing and intermediate heat treatment, the sliding friction between the wire and the die surface is large during the processing, the surface quality is not easy to guarantee, and the wire is prone to breakage during the processing, so the processing difficulty is high, the production efficiency is low, and the production cost is high. A kind of A100 ultra-high strength steel wire for additive manufacturing and its cold processing method are provided. The present invention mainly uses the rotary forging drawing + bright annealing process to replace the traditional fixed die wire drawing + annealing pickling process. The rotary forging drawing can reduce the deformation pass and reduce the production cost. The appearance size of the wire produced by the rotary forging process is accurate and the surface quality is good; the bright annealing process avoids the secondary oxidation of the wire during the annealing process, and the wire after annealing does not need to be pickled, avoiding the environmental pollution caused by pickling. The appearance size accuracy of the A100 ultra-high strength steel wire for additive manufacturing produced by the method of the present invention is ±0.02mm, the surface is smooth, and there are no external surface defects such as pits, cracks, scratches, etc., which meets the technical requirements for the use of A100 ultra-high strength steel wire for additive manufacturing. The invention can stably produce the product with high dimensional accuracy, good surface quality and superior performance.

[0005] The technical means adopted by the present invention are as follows:

[0006] The invention discloses an A100 ultra-high strength steel wire material for additive manufacturing, which is a material obtained by bright annealing, rotary forging, drawing and tension straightening.

[0007] The present invention also provides a cold working method of A100 ultra-high strength steel wire for additive manufacturing, comprising the following steps:

[0008] S1. Using A100 ultra-high strength steel hot-rolled coil as raw material, removing the surface oxide layer;

[0009] S2, placing the A100 ultra-high strength steel hot-rolled coil processed in step S1 in a hydrogen annealing furnace for bright annealing;

[0010] S3, subjecting the material obtained after the annealing treatment in step S2 to multiple passes of rotary forging, drawing and bright annealing to obtain a wire blank;

[0011] S4, subjecting the wire blank obtained in step S3 to a final rotary forging and drawing process to obtain a finished wire product;

[0012] S5, placing the finished wire obtained in step S4 in a hydrogen annealing furnace for bright annealing;

[0013] S6. Perform tension straightening on the wire obtained in step S5 to obtain A100 ultra-high strength steel wire.

[0014] Furthermore, the specific steps of step S1 are as follows:

[0015] The diameter The A100 ultra-high strength steel hot-rolled coil is peeled to remove the oxide layer on the surface of the hot-rolled coil.

[0016] Furthermore, in step S2, the annealing temperature ranges from 650°C to 700°C, the annealing time is from 10h to 12h, and the furnace is cooled to room temperature after the annealing is completed.

[0017] Furthermore, the specific steps of step S3 are as follows:

[0018] S31, performing rotary forging and drawing on the material annealed in step S2;

[0019] S32, placing the material after rotary forging and drawing in step S31 in a hydrogen annealing furnace for bright annealing to remove processing stress;

[0020] S33, repeating steps S31 and S32 for multiple times on the material annealed in step S32, until the wire is forged to a size close to the final size, thereby obtaining a wire blank.

[0021] Furthermore, in the step S3, the deformation of the material after each rotary forging and drawing pass is ≤35%, and the rotary forging feed speed in each rotary forging and drawing pass is ≤10 mm / s.

[0022] Furthermore, in step S32, the annealing temperature ranges from 650°C to 700°C, the annealing time is 1h to 2h, and the furnace is cooled to room temperature after the annealing is completed.

[0023] Furthermore, in the step S4, the deformation of the material after the last rotary forging and drawing is ≤25%, and the rotary forging feeding speed of the last rotary forging and drawing is ≤6 mm / s.

[0024] Furthermore, in step S5, the annealing temperature ranges from 650°C to 700°C, the annealing time is 1h to 2h, and the furnace is cooled to room temperature after the annealing is completed.

[0025] Furthermore, in step S6, the diameter of the A100 ultra-high strength steel wire obtained is

[0026] Compared with the prior art, the present invention has the following advantages:

[0027] The A100 ultra-high strength steel wire for additive manufacturing and its cold processing method provided by the present invention adopt a rotary forging drawing + bright annealing process to replace the traditional fixed die wire drawing + annealing pickling process. The rotary forging drawing can reduce the deformation times and reduce the production cost. The wire produced by the rotary forging process has accurate appearance dimensions and good surface quality. The bright annealing process avoids the secondary oxidation of the wire during the annealing process. The wire after annealing does not need to be pickled, thus avoiding the environmental pollution caused by pickling. The A100 ultra-high strength steel wire for additive manufacturing produced by the method of the present invention has an appearance dimension accuracy of ±0.02mm, a smooth surface, and no external surface defects such as pits, cracks, and scratches, meeting the technical requirements for the use of A100 ultra-high strength steel wire for additive manufacturing.

[0028] In summary, the application of the technical solution of the present invention can solve the problems of traditional wire cold drawing using a production process of multiple fixed die drawing and intermediate heat treatment, large sliding friction between the wire and the die surface during processing, difficult to ensure surface quality, and easy to break during processing, resulting in high processing difficulty, low production efficiency and high production cost.

[0029] Based on the above reasons, the present invention can be widely promoted in the fields of preparation of wire materials for additive manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0031] Figure 1Schematic diagram of the cold working method of A100 ultra-high strength steel wire for additive manufacturing according to the present invention. DETAILED DESCRIPTION

[0032] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] like Figure 1 As shown, the present invention provides a cold processing method of A100 ultra-high strength steel wire for additive manufacturing, which can stably produce the steel with high dimensional accuracy, good surface quality of the finished product and excellent performance.

[0035] The cold working method of the A100 ultra-high strength steel wire for additive manufacturing comprises the following steps:

[0036] a. The diameter The A100 ultra-high strength steel hot rolled coil is peeled to remove the oxide layer on the surface of the hot rolled coil;

[0037] b. Place the peeled A100 ultra-high strength steel hot-rolled coil in a hydrogen annealing furnace for bright annealing at a temperature range of 650°C to 700°C for 10h to 12h. After annealing, cool the furnace to room temperature.

[0038] c. The material annealed in step b is subjected to rotary forging and drawing, wherein the deformation amount of each rotary forging and drawing pass is ≤35%, and the rotary forging feed speed is ≤10mm / s;

[0039] d. Place the material after rotary forging in step c in a hydrogen annealing furnace for bright annealing to remove processing stress. The annealing temperature range is 650° C. to 700° C. The annealing time is 1 h to 2 h. After the annealing is completed, the furnace is cooled to room temperature.

[0040] e. Repeating steps c to d for the material annealed in step d until the wire is forged to a size close to the final size, and then performing rotary forging and drawing with a deformation amount of ≤25% as the final deformation, and the rotary forging feed speed is ≤6 mm / s;

[0041] f. Repeat step d with the material in step e, and then perform tension straightening to finally obtain a A100 ultra-high strength steel wire.

[0042] The present invention adopts a rotary forging drawing + bright annealing process to replace the traditional fixed die wire drawing + annealing pickling process. The rotary forging drawing can reduce the deformation times and reduce the production cost. The wire produced by the rotary forging process has accurate appearance dimensions and good surface quality. The bright annealing process avoids the secondary oxidation of the wire during the annealing process. The annealed wire does not need to be pickled, thus avoiding the environmental pollution caused by pickling. The A100 ultra-high strength steel wire for additive manufacturing produced by the method of the present invention has an appearance dimension accuracy of ±0.02mm, a smooth surface, and no external surface defects such as pits, cracks, and scratches, meeting the technical requirements for the use of A100 ultra-high strength steel wire for additive manufacturing.

[0043] Example 1

[0044] Diameter The A100 hot rolled coil is forged in 9 passes to obtain a diameter of The steps for making A100 ultra-high strength steel wire for additive manufacturing are as follows:

[0045] a. The A100 hot-rolled coil is peeled to remove the oxide layer on the surface of the hot-rolled coil;

[0046] b. Place the peeled material in step a in a hydrogen annealing furnace for bright annealing at a temperature of 680° C. for 12 h. After annealing, cool the furnace to room temperature.

[0047] c. The annealed material in step b is subjected to rotary forging and drawing, with a rotary forging feed speed of 6 mm / s and a deformation amount of 33% to obtain a diameter of Wire blank;

[0048] d. Place the material in step c in a hydrogen annealing furnace for bright annealing at a temperature of 680° C. for 2 h, and cool the furnace to room temperature after annealing.

[0049] e. Repeat steps c to d until a diameter of A100 ultra-high strength steel wire billet;

[0050] The deformation amount of each pass and the diameter after rotary forging are shown in Table 1:

[0051] Table 1 Deformation of A100 ultra-high strength steel in each pass of rotary forging

[0052] path 1 2 3 4 5 6 7 8 Deformation (%) 33.5 34.1 33.8 31.3 31.5 33.9 32.7 33.9 Forged size (mm) 5.3 4.3 3.5 2.9 2.4 2.0 1.6 1.3

[0053] f. The diameter of step e is The wire blank is forged and drawn, the feed speed is 4mm / s, the deformation is 15%, and the diameter is obtained. A100 finished wire products;

[0054] g. The diameter of step f is The A100 finished wire is placed in a hydrogen annealing furnace for bright annealing at a temperature of 680°C for 2 hours. After annealing, the furnace is cooled to room temperature.

[0055] h. The A100 wire described in step g is tension straightened to finally obtain a wire having a diameter of A100 ultra-high strength steel wire.

[0056] The finished wire material described in Example 1 has been quality tested, and the appearance dimension deviation is ±0.01 mm, the appearance is smooth, and there are no defects such as pits, cracks, scratches, etc., which meets the use conditions of wire materials for additive manufacturing.

[0057] Example 2

[0058] Diameter The A100 hot rolled coil is forged in 7 passes to obtain a diameter of The steps for making A100 ultra-high strength steel wire for additive manufacturing are as follows:

[0059] a. The A100 hot-rolled coil is peeled to remove the oxide layer on the surface of the hot-rolled coil;

[0060] b. Place the peeled material in step a in a hydrogen annealing furnace for bright annealing at a temperature of 680° C. for 12 h. After annealing, cool the furnace to room temperature.

[0061] c. The annealed material in step b is subjected to rotary forging and drawing, with a rotary forging feed speed of 6 mm / s and a deformation amount of 34% to obtain a diameter of Wire blank;

[0062] d. Place the material in step c in a hydrogen annealing furnace for bright annealing at a temperature of 680° C. for 2 h, and cool the furnace to room temperature after annealing.

[0063] e. Repeat steps c to d until a diameter of A100 ultra-high strength steel wire billet;

[0064] The deformation amount of each pass and the diameter after rotary forging are shown in Table 2:

[0065] Table 2 Deformation of A100 ultra-high strength steel in each pass of rotary forging

[0066] path 1 2 3 4 5 6 Deformation (%) 34 35 35 34 31 35 Forged size (mm) 6.5 5.2 4.2 3.4 2.8 2.2

[0067] f. The diameter of step e is The wire blank is forged and drawn, the feed speed is 4mm / s, the deformation is 17%, and the diameter is obtained. A100 finished wire products;

[0068] g. The diameter of step f is The A100 finished wire is placed in a hydrogen annealing furnace for bright annealing at a temperature of 680°C for 2 hours. After annealing, the furnace is cooled to room temperature.

[0069] h. The A100 wire described in step g is tension straightened to finally obtain a wire having a diameter of A100 ultra-high strength steel wire.

[0070] The finished wire material described in Example 2 has been quality inspected, and the appearance dimension deviation is ±0.01 mm, the appearance is smooth, and there are no defects such as pits, cracks, scratches, etc., which meets the use conditions of wire materials for additive manufacturing.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A cold working method for A100 ultra-high strength steel wire for additive manufacturing, characterized in that: The steps include: S1. Using A100 ultra-high strength steel hot-rolled coil as raw material, removing the surface oxide layer; S2, placing the A100 ultra-high strength steel hot-rolled coil processed in step S1 in a hydrogen annealing furnace for bright annealing; S3, subjecting the material obtained after the annealing treatment in step S2 to multiple passes of rotary forging, drawing and bright annealing to obtain a wire blank; S4, subjecting the wire blank obtained in step S3 to a final rotary forging and drawing process to obtain a finished wire product; S5, placing the finished wire obtained in step S4 in a hydrogen annealing furnace for bright annealing; S6. Perform tension straightening on the wire obtained in step S5 to obtain A100 ultra-high strength steel wire.

2. The cold working method of A100 ultra-high strength steel wire for additive manufacturing according to claim 1, characterized in that: The specific steps of step S1 are as follows: The A100 ultra-high strength steel hot-rolled coil with a diameter of φ6mm-φ8mm is peeled to remove the oxide layer on the surface of the hot-rolled coil.

3. The cold working method of A100 ultra-high strength steel wire for additive manufacturing according to claim 1, characterized in that: In step S2, the annealing temperature ranges from 650°C to 700°C, the annealing time is from 10h to 12h, and the furnace is cooled to room temperature after the annealing is completed.

4. The cold working method of A100 ultra-high strength steel wire for additive manufacturing according to claim 1, characterized in that: The specific steps of step S3 are as follows: S31, performing rotary forging and drawing on the material annealed in step S2; S32, placing the material after rotary forging and drawing in step S31 in a hydrogen annealing furnace for bright annealing to remove processing stress; S33, repeating steps S31 and S32 for multiple times on the material annealed in step S32, until the wire is forged to a size close to the final size, thereby obtaining a wire blank.

5. The cold working method of A100 ultra-high strength steel wire for additive manufacturing according to claim 1 or 4, characterized in that: In the step S3, the deformation of the material after each rotary forging and drawing pass is ≤35%, and the rotary forging feed speed in each rotary forging and drawing pass is ≤10 mm / s.

6. The cold working method of A100 ultra-high strength steel wire for additive manufacturing according to claim 4, characterized in that: In the step S32, the annealing temperature ranges from 650°C to 700°C, the annealing time is 1 hour to 2 hours, and the furnace is cooled to room temperature after the annealing is completed.

7. The cold working method of A100 ultra-high strength steel wire for additive manufacturing according to claim 1, characterized in that: In the step S4, the deformation of the material after the last rotary forging and drawing is ≤25%, and the rotary forging feeding speed of the last rotary forging and drawing is ≤6 mm / s.

8. The cold working method of A100 ultra-high strength steel wire for additive manufacturing according to claim 1, characterized in that: In step S5, the annealing temperature ranges from 650°C to 700°C, the annealing time is 1 hour to 2 hours, and the furnace is cooled to room temperature after the annealing is completed.

9. The cold working method of A100 ultra-high strength steel wire for additive manufacturing according to claim 1, characterized in that: In the step S6, the diameter of the obtained A100 ultra-high strength steel wire is φ1.0 mm to φ2.0 mm.