Non-oriented silicon steel and high-clean production method thereof
By controlling impurity elements and temperature in the production of non-oriented silicon steel, reducing inclusion precipitation, the problem of inclusions affecting magnetic properties is solved, and a non-oriented silicon steel product with high cleanliness and stable properties is achieved.
Patent Information
- Application Number
- CN202211719342.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-12-30
AI Technical Summary
In the production process of existing non-oriented silicon steel, inclusions such as sulfur-based compounds, carbon-nitrogen-based compounds affect the magnetic properties, resulting in increased iron loss and changes in magnetic domain structure, making it difficult to achieve high cleanliness and stable performance.
Using specific process flows, including iron desulfurization, converter smelting, vacuum refining, continuous casting and rolling, control impurities at extremely low levels, reduce inclusion precipitation through superheat and temperature control, and promote precipitate ablation during the annealing process. Improve the cleanliness of finished products.
The number and size of inclusions such as oxides, sulfides and carbon nitrides is significantly reduced, iron loss is reduced, and the magnetic properties and quality of non-oriented silicon steel are improved, and the iron loss is reduced by 0.2~0.6W/kg.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel material preparation, and relates to non-oriented silicon steel and a high-clean production method thereof. Background Art
[0002] The magnetic properties of non-oriented silicon steel mainly depend on the ferrite grain size, crystal texture and the distribution of inclusions in the steel. The inclusions in the steel mainly include the following categories: CaO, Al2O3, SiO2 and other oxygen inclusions; CaS, MnS, Cu x Sulfur-based compounds such as S; carbon-nitrogen-based compounds such as TiN, Ti(CN), AlN, V(CN), and Zr(CN). Under industrial production conditions, the inclusions that have a greater impact on magnetic properties are mainly sulfur-based compounds and carbon-nitrogen-based compounds. These inclusions are formed during the casting, solidification, slab heating and rolling of molten steel, and are small in size and dispersed in distribution.
[0003] The main reasons why these inclusions affect the magnetic properties of non-oriented silicon steel are: (1) The inclusions are small in size and close to the size of the magnetic domain wall, which hinders the grain growth during the final annealing process and leads to increased iron loss of the material; (2) Inclusions cause the crystal lattice to be distorted, and the dislocation density around the inclusions increases, causing an additional internal stress field, resulting in an increase in static magnetic energy and magnetoelastic properties, changes in the magnetic domain structure, and difficulty in magnetization. Summary of the invention
[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a non-oriented silicon steel and a high-clean production method thereof, so as to improve the magnetic properties of the silicon steel and ensure the performance stability.
[0005] To achieve the above-mentioned purpose, an embodiment of the present invention provides a high-clean production method for non-oriented silicon steel, which comprises the following steps:
[0006] 1) Hot metal desulfurization: Use hot metal with Si 0.25-0.65%, S≤0.04%, Nb≤0.0015%, V≤0.035%, Ti≤0.050%, Mo≤0.0010%, As≤0.0010%, Zr≤0.0010%, Cu≤0.0035% by mass percentage to carry out KR desulfurization, and the slag removal rate after desulfurization is ≥97% and S≤0.0015%;
[0007] 2) Converter smelting: the desulfurized molten iron in step 1 is smelted in a converter, the smelting end point temperature is 1640-1680°C, the O content is 0.05-0.085%, and the slag is controlled by a slag stopper and a slide plate during the steel tapping process;
[0008] 3) Vacuum refining: After vacuum decarburization, ferrosilicon alloy is first added for deoxidation, and then metal manganese is added for alloying. After a cycle of 3 to 5 minutes, metal aluminum is added for final deoxidation. At the same time, silicon carbide is added to the slag surface of the ladle to deoxidize the slag to produce a low-basicity calcium aluminosilicate slag system. After all chemical components meet the standards, the net cycle treatment time is ≥10 minutes, and then the air is broken and the steel is tapped;
[0009] 4) Continuous casting: The superheat during the entire casting process is controlled at 30±5℃, the crystallizer liquid level fluctuation is controlled at ±2mm, the crystallizer electromagnetic stirring frequency is 5-10Hz, and the current is 400-600A;
[0010] 5) Rolling: first, the continuous casting billet obtained in step 4 is heated in a heating furnace, the heating furnace temperature is 1090-1130°C; then, hot rolling and coiling are performed to obtain hot-rolled coils, the final rolling temperature is 860-900°C, the coiling temperature is 650-660°C, and the thickness of the hot-rolled coils is 2.1-2.5 mm; then, cold rolling is performed to obtain cold-rolled strips with a thickness of 0.35-0.5 mm.
[0011] Preferably, the production method further comprises the following steps:
[0012] 6) Annealing: The cold-rolled strip obtained in step 5 is subjected to finished product annealing in an annealing furnace, the annealing temperature heating rate is 25-35°C / s, the soaking temperature is 930-960°C, and the holding time is 60-80s.
[0013] Preferably, in step 2, the amount of steel retained in the later stage of converter steel tapping is 1.5 to 3.5 tons.
[0014] Preferably, in step 1, the molten iron is made of silicon steel scrap and electrical steel scrap, and the scrap contains S≤0.0035%, Nb≤0.003%, V≤0.003%, Ti≤0.003%, Mo≤0.0050%, As≤0.0050%, and Cu≤0.008%.
[0015] Preferably, in the ferrosilicon alloy of step 3, S≤0.005%, C≤0.005%, Ti≤0.0035%, and the rest are Si and Fe.
[0016] Preferably, in the metal manganese in step 3, S≤0.015%, C≤0.010%, Ti≤0.008%, and the rest are Mn and Fe.
[0017] Preferably, the vacuum furnace and ladle used in step 3, and the refractory materials used for continuous casting in step 4, are all zirconium-free refractory materials.
[0018] Preferably, the ladle slag line used in step 3 is made of magnesia-chromium ultra-low carbon bricks, and the stopper rod slag line and the invasive nozzle slag line used for continuous casting in step 4 are both made of magnesia-alumina spinel, with a ZrO2 content of ≤0.5%.
[0019] In order to achieve the above-mentioned purpose of the invention, one embodiment of the present invention provides a non-oriented silicon steel, which is prepared by the production method.
[0020] Preferably, the surface density of inclusions with a size of 0.1 μm or more in the cold-rolled silicon steel sheet of the non-oriented silicon steel is ≤150 / mm 2 .
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: on the one hand, the impurity elements that are not easily oxidized are controlled at a relatively low level in the molten iron stage; at the same time, in converter smelting, the high oxidizability can remove the easily oxidized elements, and the slag control during steel tapping can reduce the entry of titanium oxide and the like into the ladle, thereby avoiding reduction and entering the molten steel during subsequent alloying, and the impurity elements are controlled at an extremely low level throughout the entire process of molten iron desulfurization, converter smelting, vacuum refining and continuous casting; on the other hand, the superheat control in continuous casting and the various temperature controls in the steel rolling process can reduce the precipitation of fine sulfides, oxides and other inclusions, and can further promote the ablation of precipitates by controlling the annealing temperature, heating rate and the like, thereby improving the cleanliness of the final product, greatly reducing the number and size of inclusions such as oxides, sulfides and carbonitrides in the finished product, and improving the performance and quality of non-oriented silicon steel. DETAILED DESCRIPTION
[0022] An embodiment of the present invention provides a production method of non-oriented silicon steel, and non-oriented silicon steel prepared by the production method.
[0023] In the chemical composition of the non-oriented silicon steel of the present invention, some harmful elements are calculated by mass percentage as follows: C≤0.0020%, S≤0.0015%, TO≤0.0015%, N≤0.0020%, Nb≤0.003%, V≤0.005%, Ti≤0.002%, and Zr≤0.003%.
[0024] The production method includes the following steps: hot metal desulfurization, converter smelting, vacuum refining, billet casting, rolling, finished product annealing, etc. The production method is described in detail below according to the following steps.
[0025] (1) Desulfurization of molten iron
[0026] Using molten iron containing Si 0.25-0.65%, S≤0.04%, Nb≤0.0015%, V≤0.035%, Ti≤0.050%, Mo≤0.0010%, As≤0.0010%, Zr≤0.0010%, and Cu≤0.0035% by mass percentage, KR desulfurization is carried out, and the slag removal rate after desulfurization is ≥97% and S≤0.0015%;
[0027] Preferably, in this step, the molten iron is made of silicon steel scrap and electrical steel scrap, and the scrap contains S≤0.0035%, Nb≤0.003%, V≤0.003%, Ti≤0.003%, Mo≤0.0050%, As≤0.0050%, and Cu≤0.008%.
[0028] (2) Converter smelting
[0029] The desulfurized molten iron in step 1 is smelted in a converter, with a smelting end point temperature of 1640-1680° C. and an O content of 0.05-0.085%. During the steel tapping process, a slag stopper and a slide plate are used to control the slag discharge;
[0030] Preferably, the amount of steel retained in the converter in the later stage of steel tapping is 1.5 to 3.5 tons to avoid slag.
[0031] (3) Vacuum refining
[0032] After vacuum decarburization, ferrosilicon alloy is first added for deoxidation, and then metal manganese is added for alloying. After a cycle of 3 to 5 minutes, metal aluminum is added for final deoxidation. At the same time, silicon carbide is added to the slag surface of the ladle to deoxidize the slag to produce a low-basicity calcium aluminosilicate slag system. After all chemical components meet the standards, the net cycle treatment time is ≥10 minutes, and then the air is broken and the steel is tapped;
[0033] Among them, in ferrosilicon alloy, S≤0.005%, C≤0.005%, Ti≤0.0035%, and the rest are Si and Fe; in metal manganese, S≤0.015%, C≤0.010%, Ti≤0.008%, and the rest are Mn and Fe;
[0034] Preferably, the vacuum furnace and ladle used in this step are made of zirconium-free refractory materials; furthermore, the ladle slag line used is made of magnesium-chromium ultra-low carbon bricks.
[0035] (4) Continuous casting
[0036] The superheat during the whole pouring process is controlled at 30±5℃, the crystallizer liquid level fluctuation is controlled at ±2mm, the crystallizer electromagnetic stirring frequency is 5-10Hz, and the current is 400-600A;
[0037] Preferably, the refractory materials used for continuous casting in this step are all zirconium-free refractory materials; furthermore, the stopper rod slag line and the intrusive nozzle slag line are both made of magnesia-aluminum spinel, and the ZrO2 content is ≤0.5%.
[0038] (5) Rolling
[0039] First, the continuous casting slab obtained in step 4 is heated in a heating furnace, the heating furnace temperature is 1090-1130° C.; then hot rolling and coiling are performed to obtain hot rolled coils, the final rolling temperature is 860-900° C., the coiling temperature is 650-660° C., and the thickness of the hot rolled coils is 2.1-2.5 mm; then cold rolling is performed to obtain cold rolled strips with a thickness of 0.35-0.5 mm;
[0040] (6) Finished product annealing
[0041] The cold-rolled strip obtained in step 5 is subjected to finished product annealing in an annealing furnace, the annealing temperature heating rate is 25-35°C / s, the soaking temperature is 930-960°C, and the holding time is 60-80s.
[0042] Compared with the prior art, the non-oriented silicon steel prepared by the production method of the present invention has a surface density of inclusions with a size of 0.1 μm or more in the cold-rolled silicon steel sheet of ≤150 pieces / mm. 2 Compared with non-oriented silicon steel with the same Si, Mn, Al, Sn and Sb contents, the magnetic properties are reduced by 0.2 to 0.6 W / kg.
[0043] The beneficial effects of the present invention are as follows: on the one hand, the impurity elements that are not easily oxidized are controlled at a relatively low level in the molten iron stage; at the same time, in converter smelting, the high oxidizability can remove the easily oxidized elements, and by controlling the slag during steel tapping, the entry of titanium oxide and the like into the ladle is reduced, thereby avoiding reduction into the molten steel during subsequent alloying, and the impurity elements are controlled at an extremely low level throughout the entire process of molten iron desulfurization, converter smelting, vacuum refining and continuous casting; on the other hand, the superheat control in continuous casting and the various temperature controls in the steel rolling process can reduce the precipitation of fine sulfides, oxides and other inclusions. In addition, the ablation of precipitates can be further promoted by controlling the annealing temperature, the heating rate and the like, thereby improving the cleanliness of the final product, greatly reducing the number and size of inclusions such as oxides, sulfides and carbonitrides in the finished product, and improving the performance and quality of non-oriented silicon steel.
[0044] The detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
[0045] The beneficial effects of the present invention are further illustrated by three embodiments below. Of course, these three embodiments are only a part of the many variations of the present invention, but not all of them.
[0046] Example 1
[0047] Provided is a non-oriented silicon steel, which is prepared by the following process.
[0048] (1) Desulfurization of molten iron
[0049] Silicon steel scrap and electrical steel scrap are used as raw materials to produce molten iron, and the scrap contains S=0.0015%, Nb=0.001%, V=0.0015%, Ti=0.002%, Mo=0.0018%, As=0.002%, and Cu=0.0068% by mass;
[0050] The obtained molten iron is subjected to KR desulfurization. Before desulfurization, the molten iron contains Si=0.25%, S=0.023%, Nb=0.0010%, V=0.026%, Ti=0.033%, Mo=0.0008%, As=0.0005%, Zr=0.0007%, and Cu=0.0027% by mass.
[0051] After desulfurization, the slagging rate is 99%, S=0.0005%;
[0052] (2) Converter smelting
[0053] The desulfurized molten iron in step 1 is smelted in a converter, with a smelting end point temperature of 1640° C. and an O content of 0.05%. During the steel tapping process, a slag stopper and a slide plate are used to control the slag discharge;
[0054] The amount of steel left in the converter at the later stage of steel tapping is 3.5t to avoid slag;
[0055] (3) Vacuum refining
[0056] After vacuum decarburization, ultra-pure ferrosilicon alloy is first added for deoxidation, and then metal manganese is added for alloying. After a 3-minute cycle, metal aluminum is added for final deoxidation. At the same time, silicon carbide is added to the slag surface of the ladle to deoxidize the slag to produce a low-basicity calcium aluminosilicate slag system. After all chemical components meet the standards, the net cycle treatment time is 15 minutes, and then the air is broken and the steel is tapped.
[0057] Among them, in ferrosilicon alloy, S=0.0035%, C=0.0028%, Ti=0.0026%, and the rest are Si and Fe; in metal manganese, S=0.011%, C=0.0085%, Ti=0.0052%, and the rest are Mn and Fe;
[0058] The vacuum furnace and ladle used in this step are both made of zirconium-free refractory materials; furthermore, the ladle slag line used is made of magnesium-chromium ultra-low carbon bricks;
[0059] (4) Continuous casting
[0060] The superheat during the whole pouring process is controlled at 30±5℃, the crystallizer liquid level fluctuation is controlled at ±2mm, the crystallizer electromagnetic stirring frequency is 5Hz, and the current is 600A;
[0061] In this step, the refractory materials used for continuous casting are all zirconium-free refractory materials; furthermore, the stopper slag line and the intrusive nozzle slag line are all made of magnesia-alumina spinel, with a ZrO2 content of 0.26%;
[0062] (5) Rolling
[0063] First, the continuous casting slab obtained in step 4 is heated in a heating furnace at a temperature of 1090° C.; then, hot rolling and coiling are performed to obtain hot-rolled coils, the final rolling temperature is 860° C., the coiling temperature is 650° C., and the thickness of the hot-rolled coils is 2.1 mm; then, cold rolling is performed to obtain cold-rolled strips with a thickness of 0.35 mm;
[0064] (6) Finished product annealing
[0065] The cold-rolled strip obtained in step 5 is subjected to finished product annealing in an annealing furnace, with an annealing temperature heating rate of 25°C / s, a soaking temperature of 930°C, and a holding time of 60s.
[0066] The thickness of the silicon steel product is 0.35mm, and the mass percentage of key harmful elements in the chemical composition is: C = 0.0013%, S = 0.0012%, TO = 0.0011%, N = 0.0016%, Nb = 0.0008%, V = 0.0013%, Ti = 0.0009%, Mo = 0.0027%, As = 0.0025%, Zr = 0.0029%, Cu = 0.0037%. The surface density of inclusions with a size of 0.1μm or more in the cold-rolled silicon steel sheet is 139 / mm 2 .
[0067] Example 2
[0068] Provided is a non-oriented silicon steel, which is prepared by the following process.
[0069] (1) Desulfurization of molten iron
[0070] Silicon steel scrap and electrical steel scrap are used as raw materials to produce molten iron, and the scrap contains S=0.0035%, Nb=0.003%, V=0.003%, Ti=0.003%, Mo=0.005%, As=0.005%, and Cu=0.008% by mass;
[0071] The obtained molten iron is subjected to KR desulfurization. Before desulfurization, the molten iron contains Si=0.25%, S=0.04%, Nb=0.0015%, V=0.035%, Ti=0.050%, Mo=0.0010%, As=0.0010%, Zr=0.0010%, and Cu=0.0035% by mass;
[0072] After desulfurization, the slagging rate is 97%, S=0.0015%;
[0073] (2) Converter smelting
[0074] The desulfurized molten iron in step 1 is smelted in a converter, with a smelting end point temperature of 1680° C. and an O content of 0.085%. During the steel tapping process, a slag stopper and a slide plate are used to control the slag discharge;
[0075] The amount of steel left in the converter at the later stage of steel tapping is 1.5t to avoid slag;
[0076] (3) Vacuum refining
[0077] After vacuum decarburization, ultra-pure ferrosilicon alloy is first added for deoxidation, and then metal manganese is added for alloying. After 5 minutes of circulation, metal aluminum is added for final deoxidation. At the same time, silicon carbide is added to the slag surface of the ladle to deoxidize the slag to produce a low-basicity calcium aluminosilicate slag system. After all chemical components meet the standards, the net circulation treatment time is 10 minutes, and then the air is broken and the steel is tapped.
[0078] Among them, in ferrosilicon alloy, S=0.005%, C=0.005%, Ti=0.0035%, and the rest are Si and Fe; in metal manganese, S=0.015%, C=0.0010%, Ti=0.008%, and the rest are Mn and Fe;
[0079] The vacuum furnace and ladle used in this step are both made of zirconium-free refractory materials; furthermore, the ladle slag line used is made of magnesium-chromium ultra-low carbon bricks;
[0080] (4) Continuous casting
[0081] The superheat during the whole pouring process is controlled at 30±5℃, the crystallizer liquid level fluctuation is controlled at ±2mm, the crystallizer electromagnetic stirring frequency is 10Hz, and the current is 400A;
[0082] In this step, the refractory materials used for continuous casting are all zirconium-free refractory materials; furthermore, the stopper slag line and the intrusive nozzle slag line are all made of magnesia-alumina spinel, with a ZrO2 content of 0.5%;
[0083] (5) Rolling
[0084] First, the continuous casting slab obtained in step 4 is heated in a heating furnace at a temperature of 1130° C.; then, hot rolling and coiling are performed to obtain hot-rolled coils, the final rolling temperature is 900° C., the coiling temperature is 660° C., and the thickness of the hot-rolled coils is 2.5 mm; then, cold rolling is performed to obtain cold-rolled strips with a thickness of 0.5 mm;
[0085] (6) Finished product annealing
[0086] The cold-rolled strip obtained in step 5 is subjected to finished product annealing in an annealing furnace, with an annealing temperature heating rate of 35°C / s, a soaking temperature of 960°C, and a holding time of 60s.
[0087] The thickness of the silicon steel product is 0.50mm, and the mass percentage of key harmful elements in the chemical composition is: C = 0.0020%, S = 0.0015%, TO = 0.0015%, N = 0.0020%, Nb = 0.002%, V = 0.002%, Ti = 0.002%, Mo = 0.0040%, As = 0.0040%, Zr = 0.005%, Cu = 0.005%. The surface density of inclusions with a size of 0.1μm or more in the cold-rolled silicon steel sheet is 150 pieces / mm 2 .
[0088] Example 3
[0089] Provided is a non-oriented silicon steel, which is prepared by the following process.
[0090] (1) Desulfurization of molten iron
[0091] Silicon steel scrap and electrical steel scrap are used as raw materials to produce molten iron, and the scrap contains S=0.0028%, Nb=0.0022%, V=0.0026%, Ti=0.0019%, Mo=0.0038%, As=0.0041%, and Cu=0.007% by mass;
[0092] The obtained molten iron is subjected to KR desulfurization. Before desulfurization, the molten iron contains Si=0.51%, S=0.033%, Nb=0.0012%, V=0.028%, Ti=0.032%, Mo=0.0007%, As=0.0007%, Zr=0.0005%, and Cu=0.0029% by mass.
[0093] After desulfurization, the slagging rate is 98%, S=0.0007%;
[0094] (2) Converter smelting
[0095] The desulfurized molten iron in step 1 is smelted in a converter, with a smelting end point temperature of 1665° C. and an O content of 0.065%. During the steel tapping process, slag stoppers and slide plates are used to control slag discharge;
[0096] The amount of steel retained in the converter at the later stage of steel tapping is 2.6t to avoid slag;
[0097] (3) Vacuum refining
[0098] After vacuum decarburization, ultra-pure ferrosilicon alloy is first added for deoxidation, and then metal manganese is added for alloying. After a 4-minute cycle, metal aluminum is added for final deoxidation. At the same time, silicon carbide is added to the slag surface of the ladle to deoxidize the slag to produce a low-basicity calcium aluminosilicate slag system. After all chemical components meet the standards, the net cycle treatment time is 11 minutes, and then the air is broken and the steel is tapped.
[0099] Among them, in ferrosilicon alloy, S=0.0042%, C=0.0039%, Ti=0.0026%, and the rest are Si and Fe; in metal manganese, S=0.0102%, C=0.0075%, Ti=0.0046%, and the rest are Mn and Fe;
[0100] The vacuum furnace and ladle used in this step are both made of zirconium-free refractory materials; furthermore, the ladle slag line used is made of magnesium-chromium ultra-low carbon bricks;
[0101] (4) Continuous casting
[0102] The superheat during the whole pouring process is controlled at 30±5℃, the crystallizer liquid level fluctuation is controlled at ±2mm, the crystallizer electromagnetic stirring frequency is 8Hz, and the current is 500A;
[0103] In this step, the refractory materials used for continuous casting are all zirconium-free refractory materials; furthermore, the stopper slag line and the intrusive nozzle slag line are all made of magnesia-alumina spinel, with a ZrO2 content of 0.35%;
[0104] (5) Rolling
[0105] First, the continuous casting slab obtained in step 4 is heated in a heating furnace at a temperature of 1100° C.; then, hot rolling and coiling are performed to obtain hot-rolled coils, the final rolling temperature is 885° C., the coiling temperature is 655° C., and the thickness of the hot-rolled coils is 2.4 mm; then, cold rolling is performed to obtain cold-rolled strips with a thickness of 0.45 mm;
[0106] (6) Finished product annealing
[0107] The cold-rolled strip obtained in step 5 is subjected to finished product annealing in an annealing furnace, with an annealing temperature heating rate of 30°C / s, a soaking temperature of 940°C, and a holding time of 70s.
[0108] The thickness of the silicon steel product is 0.45mm, and the mass percentage of key harmful elements in the chemical composition is: C = 0.0016%, S = 0.0008%, TO = 0.0010%, N = 0.0013%, Nb = 0.0011%, V = 0.0015%, Ti = 0.0009%, Mo = 0.0022%, As = 0.0025%, Zr = 0.0036%, Cu = 0.0029%. The surface density of inclusions with a size of 0.1μm or more in the cold-rolled silicon steel sheet is 129 / mm 2 .
[0109] Compared with non-oriented silicon steels with the same Si, Mn, Al, Sn and Sb contents, the non-oriented silicon steels of Examples 1 to 3 have more excellent and stable magnetic properties, and the iron loss is reduced by 0.2 to 0.6 W / kg.
Claims
1. A high-clean production method for non-oriented silicon steel, characterized in that: The following steps are included: 1) Hot metal desulfurization: Use hot metal with Si 0.25~0.65%, S≤0.04%, Nb≤0.0015%, V≤0.035%, Ti≤0.050%, Mo≤0.0010%, As≤0.0010%, Zr≤0.0010%, Cu≤0.0035% by mass percentage for KR desulfurization. After desulfurization, the slag removal rate is ≥97% and S≤0.0015%; 2) Converter smelting: The desulfurized molten iron in step 1 is smelted in a converter, with a smelting end point temperature of 1640-1680°C and an O content of 0.05-0.085%. During the steel tapping process, slag stoppers and slide plates are used to control slag discharge; 3) Vacuum refining: After vacuum decarburization, ferrosilicon alloy is first added for deoxidation, and then metal manganese is added for alloying. After a cycle of 3-5 minutes, metal aluminum is added for final deoxidation. At the same time, silicon carbide is added to the slag surface of the ladle to deoxidize the slag to produce a low-basicity calcium aluminosilicate slag system. After all chemical components meet the standards, the net cycle treatment time is ≥10 minutes, and then the air is broken and the steel is tapped; 4) Continuous casting: The superheat during the entire casting process is controlled at 30±5℃, the crystallizer liquid level fluctuation is controlled at ±2mm, the crystallizer electromagnetic stirring frequency is 5-10Hz, and the current is 400-600A; 5) Rolling: firstly, the continuous casting slab obtained in step 4 is heated in a heating furnace, the heating furnace temperature is 1090-1130°C; then, hot rolling and coiling are performed to obtain hot-rolled coils, the final rolling temperature is 860-900°C, the coiling temperature is 650-660°C, and the thickness of the hot-rolled coils is 2.1-2.5mm; then, cold rolling is performed to obtain cold-rolled strips with a thickness of 0.35-0.5mm; 6) Annealing: The cold-rolled strip obtained in step 5 is subjected to finished product annealing in an annealing furnace, the annealing temperature heating rate is 25-35°C / s, the soaking temperature is 930-960°C, and the holding time is 60-80s; The surface density of inclusions with a size of 0.1 μm or more in the cold-rolled silicon steel sheet of the non-oriented silicon steel is ≤150 / mm 2 .
2. The high-clean production method for non-oriented silicon steel according to claim 1, characterized in that: The heating furnace temperature is 1090-1100°C, or greater than 1100°C and less than 1130°C; The final rolling temperature is between 860 and 885°C, or greater than 885°C and less than 900°C; The coiling temperature is between 650 and 655°C, or greater than 655°C and less than 660°C; The soaking temperature during annealing is 930-940°C, or greater than 940°C and less than 960°C.
3. The high-clean production method for non-oriented silicon steel according to claim 1, characterized in that: In step 2, the amount of steel retained in the converter at the later stage of steel tapping is 1.5~3.5t.
4. The high-clean production method for non-oriented silicon steel according to claim 1, characterized in that: In the ferrosilicon alloy of step 3, S≤0.005%, C≤0.005%, Ti≤0.0035%, and the rest are Si and Fe.
5. The high-clean production method for non-oriented silicon steel according to claim 1, characterized in that: The vacuum furnace and ladle used in step 3, as well as the refractory materials used for continuous casting in step 4, are all made of zirconium-free refractory materials.
6. The high-clean production method for non-oriented silicon steel according to claim 1, characterized in that: The ladle slag line used in step 3 is made of magnesia-chromium ultra-low carbon bricks, and the stopper slag line and invasive nozzle slag line used for continuous casting in step 4 are both made of magnesia-alumina spinel, with a ZrO2 content of ≤0.5%.
7. A non-oriented silicon steel, characterized in that: The method is prepared by the production method according to any one of claims 1 to 6.