A porous ceramic based on purple pottery waste and a preparation method thereof
By using Jianshui purple pottery waste, clay and glass powder to prepare porous ceramics, the problem of high cost and inability to reuse porous ceramic materials in wastewater treatment is solved, and effective filtration and adsorption of various pollutants in wastewater and ceramic materials are achieved. The reuse of the company has important significance for green and sustainable development.
Patent Information
- Application Number
- CN202310194195.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-02
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-03-02
AI Technical Summary
In the existing wastewater treatment, porous ceramic materials are cost-effective, have low treatment efficiency and cannot be reused. The traditional pore-making methods are complex and may produce toxic and harmful substances.
Jianshui purple pottery waste is used as pore-making agent to make porous ceramic material by mixing it with Jianshui clay and glass powder. After appropriate extrusion and high-temperature calcination, porous ceramics with good filtration and adsorption capabilities are formed.
It realizes effective filtration and adsorption of chemical oxygen demand, hexavalent chromium, cadmium, lead and methyl blue in wastewater, and reuse of ceramic materials through high-temperature decomposition, reducing the preparation cost and avoiding the generation of toxic substances. Expand the application value of purple pottery waste.
Smart Images

Figure CN116178041B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramics, and in particular relates to a porous ceramic based on purple pottery waste and a preparation method thereof. The porous ceramic has a water filtering function. Background Art
[0002] Water pollution is a very serious and urgent problem faced by mankind in the process of sustainable development. At present, the main problems faced by sewage treatment are: the preparation cost of sewage filtration materials is too high, the treatment efficiency is low and it cannot be reused. The materials used for sewage treatment are generally porous carbon materials, cotton fiber materials and inorganic ceramic glass materials.
[0003] Porous ceramics have the characteristics of high mechanical strength, corrosion resistance, high temperature and high pressure resistance, etc. There are many preparation methods, and adding pore-forming agents is one of the commonly used methods. This method has the following problems: the pore-forming agent is expensive, the additives may produce toxic and harmful substances, and the pore-forming method is complicated and cumbersome. Among the porous ceramic materials currently used for sewage treatment, hexagonal boron nitride porous materials and cordierite porous materials have better treatment effects, but there are also problems such as high raw material prices and high energy consumption caused by high-temperature calcination.
[0004] Jianshui purple pottery is a traditional daily-use ceramic produced in Jianshui County, Yunnan Province. It is currently mainly used as tea sets, decorative ornaments, cooking utensils, etc. In the production process of purple pottery, defective waste often occurs. These wastes have always been directly discarded, which not only occupies land but also has the potential to injure people and animals. The raw materials of Jianshui purple pottery are cheap, but they are not well utilized. Summary of the invention
[0005] Through experimental testing, it is found that Jianshui purple pottery material has a good filtering and adsorption effect on chemical oxygen demand (COD), hexavalent chromium, cadmium, lead, methyl blue and other substances in sewage. Therefore, the inventor uses purple pottery waste as a pore-forming agent to manufacture porous ceramic materials for sewage filtration, thereby completing the present invention, and the porous ceramics of the present invention can be reused, which has important application value and significance.
[0006] Therefore, in one aspect, the present invention provides a method for preparing a porous ceramic based on purple pottery waste, the method comprising:
[0007] 1) Weigh Jianshui pottery clay, add water to soften it, add purple pottery waste and glass powder to make clay;
[0008] 2) kneading the clay material evenly, squeezing it appropriately to expel air bubbles, and forming porous clay;
[0009] 3) forming the porous clay into a pot shape or a pottery ball by throwing, and trimming the pot body after it is half dry, adjusting the wall thickness of the pot body to 2-5 mm, or the diameter of the pottery ball to 1 cm;
[0010] 4) After the green body is dried, it is calcined to 1100° C., kept at 1100° C. for 30 minutes, and then cooled to room temperature to form a porous ceramic.
[0011] Furthermore, in step 1), the Jianshui pottery clay is made from pottery clay raw materials in Jianshui County, Yunnan Province, and has a mesh size of 150-250 meshes.
[0012] Furthermore, in step 1), the weight ratio of the Jianshui pottery clay to the purple pottery waste is 700:40-60, preferably 700:60.
[0013] Furthermore, in step 1), the maximum diameter of the purple pottery waste is less than 3 mm, and preferably, the fineness of the purple pottery waste is within 30 meshes.
[0014] Furthermore, in step 3), the wall thickness of the can-shaped body is adjusted to 2-3 mm.
[0015] In another aspect, the present invention relates to a porous ceramic obtained by the above preparation method.
[0016] Furthermore, the pores of the porous ceramic are evenly distributed.
[0017] In still another aspect, the present invention relates to use of the porous ceramic in sewage treatment.
[0018] Furthermore, in the application, the porous ceramic absorbs organic waste, hexavalent chromium, cadmium, and lead in sewage.
[0019] Furthermore, the porous ceramic adsorbs methyl blue or organic matter similar to methyl blue. Preferably, after the adsorption is saturated, the porous ceramic is calcined to 600-700° C. to decompose the adsorbed organic matter at high temperature, so that the porous ceramic can be reused.
[0020] Technical Effects
[0021] The present invention develops a new ceramic filtration material using Jianshui purple pottery waste and clay. Compared with the porous materials made of hexagonal boron nitride and cordierite, which have complex production processes and high costs and are currently more commonly used, the porous ceramic material made of Jianshui purple pottery waste and clay has a simple production method, low cost, and strong filtration and adsorption effects. It not only prepares filter materials that can be effectively used for sewage treatment, but also realizes the recycling of purple pottery waste, comprehensively expands the application of Jianshui purple pottery in new materials, and has important application value for green and sustainable development.
[0022] In addition, Jianshui purple pottery waste is non-toxic and harmless, and no toxic or harmful substances are produced during the high-temperature calcination process. It can be used as a pore-forming agent in purple pottery mud to increase the pore size of purple pottery. Experimental tests have found that Jianshui purple pottery materials have a good filtration and adsorption effect on chemical oxygen demand (COD), hexavalent chromium, cadmium, lead, and methyl blue in sewage, especially when adsorbing organic substances such as methyl blue. After saturation, it can be decomposed by calcination at high temperature, and the porous ceramics can be reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The porous ceramic material tank body prepared in Example 1;
[0024] Figure 2 The porous ceramic material tank body prepared in Example 2;
[0025] Figure 3 The porous ceramic material spherical filter column prepared in Example 3;
[0026] Figure 4 The porous ceramic material tank body prepared in Example 4;
[0027] Figure 5 The porous ceramic material tank body prepared in Example 5;
[0028] Figure 6 In the methyl blue filtration experiment of Experimental Example 2, the tank body began to wet after the filtration experiment was carried out for 3-5 minutes;
[0029] Figure 7 In the methyl blue filtration experiment of Experimental Example 2, the outer wall of the tank began to change from white to light color after the filtration experiment was carried out for 21 minutes;
[0030] Figure 8 In the methyl blue filtration experiment of Experimental Example 2, after the filtration experiment was carried out for 70-80 minutes, the outer wall of the tank changed from white to dark blue as a whole;
[0031] Fig. 9 This is a comparison chart of the methyl blue solution collected from the tank after the filtration experiment was performed for 6.5 hours in the methyl blue filtration experiment of Experimental Example 2 and the methyl blue solution that was not filtered;
[0032] Fig.10 In the methyl blue filtration experiment of Experimental Example 2, after the filtration is completed, the porous ceramic tank body is re-fired to 600-700° C. and then naturally cooled. DETAILED DESCRIPTION
[0033] The following describes several preferred embodiments of the present invention with reference to the drawings in the specification, so that the technical content is clearer and easier to understand. The present invention can be embodied in many different forms of embodiments, and the protection scope of the present invention is not limited to the embodiments mentioned in the text.
[0034] Example 1
[0035] Steps: Weigh 700g Jianshui clay and add a small amount of water to soften it, add 60g purple pottery waste and 15g glass powder, knead the clay evenly, and squeeze it properly to remove bubbles. Shape the porous clay into a pot shape by throwing, trim the body after it is half dry, adjust the wall thickness of the body to 2-3mm, calcine the body to 1100℃ after it is dried, keep it at 1100℃ for 30 minutes, and then cool it to room temperature.
[0036] Photo of porous ceramics Figure 1 The filtration rate of the pot-shaped porous ceramic prepared in Example 1 was 3.49 mL / h when the filtration test was performed with distilled water.
[0037] Example 2
[0038] Steps: Weigh 700g Jianshui clay and add a small amount of water to soften it, add 40g purple pottery waste and 15g glass powder, knead the clay evenly, and squeeze it properly to remove bubbles. Shape the porous clay into a pot shape by throwing, trim the body after it is half dry, adjust the wall thickness of the body to 2-3mm, calcine the body to 1100℃ after it is dried, keep it at 1100℃ for 30 minutes, and then cool it to room temperature.
[0039] Photo of porous ceramics Figure 2 As shown. The filtration test was carried out with distilled water, and the filtration rate of the pot-shaped porous ceramic prepared in Example 2 was 2 mL / h. Compared with Example 1, it can be seen that the filtration rate of the porous ceramic will be accelerated by appropriately adding more purple pottery waste to the porous clay.
[0040] Example 3
[0041] Steps: Weigh 700g of Jianshui clay and add a small amount of water to soften it, add 60g of purple pottery waste and 15g of glass powder, knead the clay evenly, and squeeze it appropriately to expel bubbles. The porous clay is made into a porous ceramic ball with a diameter of 1cm. After the green body is dried, it is calcined to 1100℃, kept at 1100℃ for 30 minutes, and then cooled to room temperature. The porous ceramic ball cooled to room temperature is placed in a cylindrical hard rubber attapulgite to make a porous ceramic ball filter column.
[0042] Photo of porous ceramics Figure 3 In the filtration test with distilled water, the porous ceramic ball filter column prepared in Example 3 has the fastest filtration speed compared with Example 1 and Example 2.
[0043] Example 4
[0044] Steps: Weigh 700g Jianshui clay and add a small amount of water to soften it, add 60g purple pottery waste and 15g glass powder, knead the clay evenly, and squeeze it properly to remove bubbles. Shape the porous clay into a pot shape by throwing, trim the body after it is half dry, adjust the wall thickness of the body to 4-5mm, calcine the body to 1100℃ after it is dried, keep it at 1100℃ for 30 minutes, and then cool it to room temperature.
[0045] Photo of porous ceramics Figure 4 The filtration test was performed with distilled water, and the filtration rate of the pot-shaped porous ceramic prepared in Example 4 was 1.11 mL / h, which was slower than that of the porous ceramic prepared in Example 1.
[0046] Example 5
[0047] Steps: Weigh 700g of Jianshui clay and add a small amount of water to soften it, add 60g of purple pottery waste with a mesh size of 30 or more but a maximum diameter of no more than 3mm (the purple pottery waste used in other embodiments of the present invention is 30 mesh or less), 15g of glass powder, knead the clay evenly, and squeeze it properly to expel bubbles. The porous clay is formed into a pot shape by throwing, and the green body is trimmed after it is half dry, and the green body wall thickness is adjusted to 4-5mm. After the green body is dried, it is calcined to 1100℃, kept at 1100℃ for 30 minutes, and then cooled to room temperature.
[0048] Photo of porous ceramics Figure 5 As shown. The pore distribution of the pot-shaped porous ceramic prepared in Example 5 is uneven, and cracks exist around the pores in some areas of the pot body. Compared with Example 4, it can be seen that the mesh number of the clinker added to the clay is greater than 30 meshes, which will easily cause local cracks and damage to the porous green body.
[0049] Experimental Example 1
[0050] Sewage filtration experiment:
[0051] The sewage was filtered using the porous ceramic material (porous ceramic tank) prepared in Example 1, and the content of the target filtrate in the sewage before and after filtration was detected. The target filtrate detection items included: chemical oxygen demand (COD), hexavalent chromium, cadmium, and lead, wherein the chemical oxygen demand (COD) and hexavalent chromium were detected in three parallel groups, and the cadmium and lead contents were detected in one group.
[0052] Take 5-6L of seriously polluted water (referring to the liquid in which the concentration of most indicators of raw water far exceeds the medium concentration of water after treatment), use filter paper to filter out the particles in the sewage to obtain the original solution, and test the content of each target water quality item in the original solution.
[0053] Make a porous ceramic tank filter (7.2 cm in diameter, 8.4 cm in height): take 0.5-1 L of the original solution, pour it into the tank and let it stand and filter for 5-10 days, collect the filtrate, and detect the content of each target detection item.
[0054] The results of the sewage filtration experiment are shown in Table 1 below:
[0055] Table 1
[0056]
[0057] According to the results of sewage filtration experiments, the porous ceramic material prepared by the present invention has a filtering and adsorption effect on chemical oxygen demand (COD), hexavalent chromium, cadmium and lead in sewage.
[0058] Experimental Example 2
[0059] Methyl blue filtration experiment
[0060] 500mL of methyl blue solution with a concentration of 0.004g / mL was prepared, 410mL of the solution was poured into a porous ceramic tank body prepared by the porous ceramic of Example 1 for filtration, and the outer surface of the porous tank body began to moisten after 3 minutes (the filtered liquid was colorless at this time), and the filtrate began to show a light blue color after 21 minutes (the color of the filtered liquid was lighter than the color of the liquid that had not been filtered in the tank body), and the white outer wall of the tank body began to turn blue from a part; the filtered liquid was dark blue after 70 minutes (the color of the filtered liquid was lighter than the color of the liquid that had not been filtered in the tank body, but darker than the color of the liquid filtered at 21 minutes); the white outer wall of the tank body turned blue as a whole after 6.5 hours; the tank body that had turned blue as a whole was placed in an electric kiln and re-fired to 600-700°C (the heating rate was 4-5°C / minute), the tank body returned to its original white color, and the filtration experiment was repeated, and the porous ceramic tank body still had a filtering and adsorption effect on methyl blue.
[0061] According to the methyl blue filtration experiment, porous ceramics have the function of filtering and adsorbing methyl blue or organic matter similar to methyl blue, and the filtration and adsorption will reach saturation. After reaching the filtration and adsorption saturation, the porous material can be calcined to 600-700℃ to decompose the adsorbed organic matter at high temperature, so as to achieve reuse.
[0062] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in the field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in the technical field based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A porous ceramic based on purple pottery waste, characterized in that: The porous ceramic is prepared by the following method, which comprises: 1) Weigh Jianshui pottery clay, soften it with water, add purple pottery waste and glass powder to make clay, wherein the weight ratio of the Jianshui pottery clay, purple pottery waste and glass powder is 700:40-60:15, and the fineness of the purple pottery waste is within 30 meshes; 2) Knead the clay material evenly, squeeze it appropriately to expel bubbles, and form porous clay; 3) forming the porous clay into a pot shape or a pottery ball by throwing, and trimming the pot body after it is half dry, so that the wall thickness of the pot body is adjusted to 2-5 mm, or the diameter of the pottery ball is adjusted to 1 cm; 4) After the green body is dried, it is calcined to 1100° C., kept at 1100° C. for 30 minutes, and then cooled to room temperature to form a porous ceramic, wherein the porous ceramic can absorb organic waste, hexavalent chromium, cadmium, lead, and methyl blue in sewage; After the adsorption is saturated, the porous ceramic is calcined to 600-700° C. to decompose the adsorbed organic matter at high temperature, so that the porous ceramic can be reused.
2. The porous ceramic according to claim 1, characterized in that In step 1), the weight ratio of the Jianshui pottery clay, the purple pottery waste and the glass powder is 700:60:
15.
3. The porous ceramic according to claim 1, characterized in that In step 3), the wall thickness of the can-shaped blank is adjusted to 2-3 mm.
4. The porous ceramic according to claim 1, characterized in that The pores of the porous ceramic are evenly distributed.
5. Use of the porous ceramic according to claim 1 in sewage treatment.
6. The use according to claim 5, characterized in that The porous ceramic absorbs organic waste, hexavalent chromium, cadmium and lead in sewage.
7. The use according to claim 5, characterized in that The porous ceramic adsorbs methyl blue.
8. The use according to claim 5, characterized in that After the adsorption is saturated, the porous ceramic is calcined to 600-700° C. to decompose the adsorbed organic matter at high temperature, so that the porous ceramic can be reused.