Uranium adsorption resin and its preparation method and application

By using the preparation method of uranyl adsorption resin in uranyl ion recovery and using polymerization and amination reaction technology, the problems of long, large consumption and high cost in the prior art uranyl ion recovery process are solved, and efficient uranium adsorption and Tolerance to the acidic environment simplifies the synthesis process and avoids the use of carcinogens.

CN116178607BActive Publication Date: 2024-12-06BEIJING RESEARCH INSTITUTE OF CHEMICAL ENGINEERING AND METALLURGY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310222776.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-09
Publication Date
2024-12-06
Estimated Expiration
2043-03-09

AI Technical Summary

Technical Problem

The prior art has problems in the recycling of uranyl ion, which has a long process, high cost, high cost, and difficult to effectively remove uranium in a highly phosphoric acid environment, and traditional resin synthesis methods are complex and carcinogens may be used.

Method used

Using a preparation method of uranium adsorption resin, styrene chloride, divinylbenzene and initiator are suspended polymerized with C5-C9 alkanes in a dispersant solution, followed by amination and with aldehyde and phosphites in The reaction was carried out under acidic catalytic conditions to obtain an uranium adsorption resin that was resistant to acid and phosphorus.

Benefits of technology

It achieves efficient adsorption of uranium, with an adsorption amount of more than 40 mg/g, and the resin has good tolerance to acidity and phosphorus, simplifying the synthesis process and avoiding the use of carcinogens.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004117374170000081
    Figure BDA0004117374170000081
Patent Text Reader

Abstract

The invention discloses a uranium adsorption resin and a preparation method and application thereof. The preparation method comprises the following steps: (1) mixing 100 to 150 parts by weight of chlorostyrene, 9.5 to 15 parts by weight of divinylbenzene and 1.2 to 2.0 parts by weight of an initiator, and then mixing with 11 to 20 parts by weight of C5-C9 chain alkane to obtain an organic phase; mixing the organic phase with 500 to 700 parts by weight of a dispersant solution, and reacting at 60 to 90° C. for 7 to 12 hours to obtain a polymer product; (2) swelling the polymer product, and then adding 50 to 80 parts by weight of ethylenediamine or trimethylamine, and reacting at 60 to 80° C. for 12 to 18 hours to obtain an amination product; (3) mixing the amination product with 300 to 500 parts by weight of an aldehyde-containing solution, 300 to 400 parts by weight of a phosphite and 80 to 150 parts by weight of an acidic catalyst, and reacting at 80 to 95° C. for 12 to 24 hours to obtain a uranium adsorption resin. The resin of the invention has a good adsorption effect on uranium in acidic phosphorus-containing and uranium-containing wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a uranium adsorption resin and a preparation method and application thereof. Background Art

[0002] Most of the waste liquid from uranium mine hydrometallurgy is acidic leaching liquid. If the uranyl ions in the acidic leaching liquid cannot be recovered and treated, it will not only cause a waste of uranium resources, but also pose a great threat to people's lives and health. Uranium is a harmful substance that will cause radioactive pollution to the environment, and after being absorbed by green plants and entering the food chain, it will accumulate in the body, destroy the hematopoietic system, and cause many diseases.

[0003] At present, the solvent extraction method is mainly used to extract uranium from wet-process phosphoric acid at home and abroad. Kerosene is used as a diluent, D2EHPA and TOPO / TRPO are used for synergistic extraction or trilaurylamine is used as an extractant, and a uranium product that meets the standards is obtained through secondary stripping. This process is long, consumes a lot of extractants, and is costly, making it difficult to promote and apply on a large scale. Due to the strong complexing ability of uranyl ions with P, it is difficult to effectively remove uranium in a high phosphoric acid environment. Therefore, it is of great practical significance to develop an effective solid adsorption material for recovering uranium from wet-process phosphoric acid.

[0004] CN106507795B discloses a sulfuric acid-resistant and chloride-resistant uranium extraction chelating resin and a synthesis method thereof, comprising the following steps: (1) swelling a styrene-divinylbenzene skeleton chlorine ball in a dichloromethane solvent, adding hexamethylenetetramine for amination, adjusting the pH value to 9-10, heating to 60-80°C, and reacting for 10-15 hours; (2) filtering, washing, and hydrolyzing with an aqueous HCl solution to obtain an ammonia ball; (3) reacting the ammonia ball with a formaldehyde solution and phosphorous acid, acidifying to a pH value of 1-2, and stirring at 90-95°C for 40-60 hours to obtain an aminophosphoric acid resin; (4) reacting the aminophosphoric acid resin with a fatty alcohol in an aqueous hydrochloric acid solution, and stirring and reacting at 75-85°C for 10-15 hours. The resin has good tolerance to sulfuric acid and chloride ions. Although it can be used to adsorb uranium, the traditional chlorine balls used in the synthesis method of the resin must be obtained through chloromethylation. The carcinogen chloromethyl ether is used in the chloromethylation process, which may bring certain risks and harms. In addition, phosphorous acid is used in the process of synthesizing the resin, and the resin needs to be obtained through multiple steps of reaction. The reaction process is relatively cumbersome. Summary of the invention

[0005] In view of this, one object of the present invention is to provide a method for preparing a uranium adsorption resin, wherein the obtained adsorption resin has good tolerance to acid and phosphorus, can selectively adsorb uranium, and has a good adsorption effect. Another object of the present invention is to provide a uranium adsorption resin prepared according to the above preparation method. Another object of the present invention is to provide an application of the uranium adsorption resin. The present invention achieves the above object through the following technical scheme.

[0006] In one aspect, the present invention provides a method for preparing a uranium adsorption resin, comprising the following steps:

[0007] (1) 100 to 150 parts by weight of chlorostyrene, 9.5 to 15 parts by weight of divinylbenzene and 1.2 to 2.0 parts by weight of an initiator are mixed, and then mixed with 11 to 20 parts by weight of a C5-C9 paraffin to obtain an organic phase; the organic phase is mixed with 500 to 700 parts by weight of a dispersant solution, and reacted at 60 to 90° C. for 7 to 12 hours to obtain a polymer product;

[0008] (2) swelling the polymer product, then adding 50 to 80 parts by weight of ethylenediamine or trimethylamine, and reacting at 60 to 80° C. for 12 to 18 hours to obtain an aminated product;

[0009] (3) mixing the amination product with 300-500 parts by weight of an aldehyde-containing solution, 300-400 parts by weight of a phosphite and 80-150 parts by weight of an acidic catalyst, and reacting at 80-95° C. for 12-24 hours to obtain a uranium adsorption resin.

[0010] In step (1), chlorostyrene, divinylbenzene, an initiator, a C5-C9 alkane and an aqueous solution containing a dispersant are uniformly mixed, and then a suspension polymerization reaction is carried out to obtain a polymer product.

[0011] In the present invention, the amount of chlorostyrene used can be 100 to 150 parts by weight, preferably 110 to 130 parts by weight. The amount of divinylbenzene used can be 9.5 to 15 parts by weight, preferably 10 to 12 parts by weight. The amount of initiator used can be 1.2 to 2.0 parts by weight, preferably 1.4 to 1.8 parts by weight.

[0012] The amount of C5-C9 paraffin can be 11 to 20 parts by weight, preferably 13 to 15 parts by weight. The present invention finds that the ratio of C5-C9 paraffin has an important influence on the pore structure of the polymer product. The addition of C5-C9 paraffin in the process of synthesizing the polymer product can be used for pore design, and a macroporous polymer product can be obtained, which is more conducive to the subsequent amination reaction and the synthesis of the resin with aminophosphite groups.

[0013] The amount of the dispersant solution used may be 500 to 700 parts by weight, preferably 550 to 650 parts by weight.

[0014] In step (1), the reaction temperature may be 60 to 90° C., preferably 70 to 80° C. The reaction time may be 7 to 12 hours, preferably 10 to 12 hours. The polymerization reaction is carried out under stirring. The stirring speed may be 100 to 200 r / min, preferably 130 to 150 r / min.

[0015] After the reaction is completed, the reaction product is filtered, washed and dried to obtain a polymer product. The filtration can be carried out by conventional filtration methods in the art. Methanol and tap water can be used for washing alternately. The drying temperature can be 40 to 60°C.

[0016] According to the preparation method of the present invention, preferably, the chlorinated styrene is p-chlorostyrene.

[0017] According to the preparation method of the present invention, preferably, the initiator is selected from one of benzoyl peroxide, azobisisobutyronitrile, and lauroyl peroxide; more preferably, the initiator is benzoyl peroxide; the dispersant solution contains 0.1-1wt% of dispersant; more preferably, the dispersant contains 0.4-0.6wt% of dispersant; the dispersant is selected from one of polyvinyl alcohol, oxidized polyvinyl alcohol, and polymaleic acid; more preferably, the dispersant is polyvinyl alcohol.

[0018] According to the preparation method of the present invention, preferably, the C5-C9 chain alkane is a mixture of straight-chain alkanes and branched-chain alkanes. In the mixture, the weight ratio of straight-chain alkanes to branched-chain alkanes can be 1:1 to 3, preferably 1:1. According to the preparation method of the present invention, preferably, the straight-chain alkane is one or more of n-pentane, n-hexane, n-heptane, and n-octane, and more preferably, the straight-chain alkane is n-hexane or n-heptane. The branched alkane is selected from one or more of branched alkanes with methyl, dimethyl or trimethyl, and more preferably, the branched alkane is selected from branched alkanes with methyl, which can be 2-methylpentane, 2-methylhexane or 2-methylheptane. According to a specific embodiment of the present invention, the branched alkane is 2-methylheptane.

[0019] In step (2), the polymer product is swollen and the pH value of the system is adjusted to above 9, and then an amination reaction is carried out with ethylenediamine or trimethylamine to obtain an aminated product. The present invention finds that the amination agent in the amination reaction has a greater influence on the adsorption capacity due to the different reaction activity and the number of bonded amino groups. In the present invention, the amination agent can be ethylenediamine or trimethylamine, preferably ethylenediamine, which is more conducive to the amination reaction and improves the adsorption capacity of the resin. The swelling agent can be one or more of toluene, ethylene dichloride, carbon tetrachloride, and tetrahydrofuran, preferably toluene or carbon tetrachloride, more preferably toluene. The amount of the swelling agent can be 120 to 200 parts by weight, preferably 140 to 160 parts by weight. The swelling time can be 30 to 60 minutes, preferably 40 to 50 minutes. The amount of ethylenediamine or trimethylamine can be 50 to 80 parts by weight, 60 to 70 parts by weight. The temperature of the amination reaction can be 60 to 80° C., preferably 60 to 70° C. The reaction time may be 12 to 18 hours, preferably 12 to 14 hours.

[0020] After the reaction is completed, the reaction product is filtered, washed and dried to obtain an aminated product. The filtration can be carried out by conventional filtration methods in the art. The product can be washed with dilute hydrochloric acid and water until it is neutral.

[0021] In step (3), the amination product is mixed with an aldehyde-containing solution, a phosphite and an acidic catalyst to react to obtain a uranium adsorption resin. The present invention finds that by introducing an acidic catalyst, aminophosphite can be directly synthesized from phosphite in one step, avoiding the traditional multi-step synthesis and simplifying the reaction process.

[0022] The amount of the aldehyde-containing solution can be 300-500 parts by weight, preferably 400-480 parts by weight. The amount of the phosphite can be 300-400 parts by weight, preferably 300-350 parts by weight; the amount of the acidic catalyst can be 80-150 parts by weight, preferably 100-120 parts by weight.

[0023] In step (3), the reaction temperature may be 80 to 95° C., preferably 85 to 90° C. The reaction time may be 12 to 24 hours, preferably 14 to 16 hours. The above dosage and reaction conditions are more conducive to the synthesis of aminophosphite.

[0024] According to the preparation method of the present invention, preferably, the phosphite is selected from dialkyl phosphites, and the carbon number of the alkyl group in the dialkyl phosphites is 1 to 5. The alkyl group may be a chain alkyl group, and the chain alkyl group may be one or more of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, and isopentyl, preferably one or more of methyl, ethyl, n-propyl, and n-butyl. According to the preparation method of the present invention, preferably, the alkyl group in the dialkyl phosphite is selected from a straight-chain alkyl group with a carbon number of 1 to 3, and the straight-chain alkyl group may be methyl, ethyl, and n-propyl, and preferably ethyl.

[0025] According to the preparation method of the present invention, preferably, the aldehyde in the aldehyde-containing solution is selected from one of formaldehyde, acetaldehyde and propionaldehyde. In some embodiments, the aldehyde is formaldehyde, and in other embodiments, the aldehyde is acetaldehyde. The acidic catalyst is selected from citric acid or hydrochloric acid; more preferably, concentrated hydrochloric acid.

[0026] On the other hand, the present invention also provides a uranium adsorption resin prepared according to the preparation method as described above, which has good tolerance to acid and phosphorus, can selectively adsorb uranium, and has a good adsorption effect, and the adsorption amount of uranium by the uranium adsorption resin is more than 40 mg / g. Preferably, the adsorption amount of uranium by the uranium adsorption resin is 50-61.6 mg / g.

[0027] In another aspect, the present invention also provides a use of the uranium adsorption resin described above in adsorbing uranium in acidic phosphorus-containing and uranium-containing wastewater. The hydrogen ion concentration in the acidic phosphorus-containing and uranium-containing wastewater is 0.2-2.0 mol / L, and the phosphate concentration is not higher than 45 g / L.

[0028] The present invention utilizes phosphite to react with a p-chloropolystyrene-divinylbenzene copolymer product with amino groups under acidic conditions to obtain a uranium adsorption resin, which has good tolerance to acid and phosphorus and has a good adsorption effect on uranium in acidic phosphorus-containing and uranium-containing wastewater. The adsorption amount of uranium by the uranium adsorption resin is above 40 mg / g. DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited thereto.

[0030] Here is the test method:

[0031] Infrared spectroscopy

[0032] The analysis was performed using a Fourier transform infrared absorption spectrometer, model TENSOR II, produced by Bruker, Germany.

[0033] Uranium adsorption performance test

[0034] The uranium adsorption resin was placed in acidic phosphorus-containing uranium-containing wastewater (solid-liquid ratio of 1:200) for adsorption test. Different acidic phosphorus-containing uranium-containing wastewaters were obtained by diluting the original solution, which was from the leaching solution of a uranium-containing phosphate mine in Guizhou. Its phosphate concentration was 40-50 g / L, sulfate concentration was 20-30 g / L, uranium concentration was 100-150 mg / L, H + The concentration is 2.8-3.6 mol / L. The hydrogen ion concentration and phosphate concentration are adjusted by adding phosphoric acid, sulfuric acid and sodium phosphate. The adsorption temperature is 15-40°C and the adsorption time is 6-10h. After adsorption, the supernatant is taken to analyze the uranium ion concentration. The uranium ion concentration is tested according to the method specified in HJ840-2017.

[0035] The calculation formula of uranium adsorption capacity is as follows:

[0036] Adsorption capacity = (V1×initial uranium ion concentration-V2×uranium ion concentration in adsorption tail liquid) / mass of adsorption resin.

[0037] Wherein, V1 is the volume of acidic phosphorus- and uranium-containing wastewater, in mL; V2 is the volume of adsorption tail liquid, in mL. The unit of uranium ion concentration is g / L. The unit of adsorption resin mass is g.

[0038] Example 1

[0039] 1.5 g of benzoyl peroxide and 120 g of p-chlorostyrene were mixed, and then 10.5 g of divinylbenzene, 6.5 g of 2-methylheptane and 6.5 g of n-hexane were added to obtain an organic phase; the organic phase was mixed with 600 ml of a 0.6 wt % polyvinyl alcohol aqueous solution, and the mixture was reacted for 10 h at a temperature of 80° C. and a stirring speed of 155 r / min to obtain a reaction product, and the reaction product was filtered, washed alternately with methanol / water, and dried at 50° C. to obtain a polymerization product.

[0040] 116 g of the polymerization product, 150 g of toluene and 65 g of ethylenediamine were mixed and reacted at 65° C. for 12 h to obtain an aminated product.

[0041] 160 g of the amination product, 450 g of formaldehyde solution, 300 g of diethyl phosphite and 100 ml of concentrated hydrochloric acid were mixed, reacted at 85° C. for 15 h, the solid was filtered out, and washed with water until neutral to obtain a uranium adsorption resin.

[0042] Comparative Example 1

[0043] 1.0 g of benzoyl peroxide and 90 g of p-chlorostyrene were mixed, and then 9 g of divinylbenzene, 7.5 g of 2-methylheptane and 2.5 g of n-hexane were added to obtain an organic phase; the organic phase was mixed with 400 ml of a 0.5 wt% polyvinyl alcohol aqueous solution, and the mixture was reacted for 10 h at a temperature of 75° C. and a stirring speed of 120 r / min to obtain a reaction product, and the reaction product was filtered, washed alternately with methanol / water, and dried at 50° C. to obtain a polymerization product.

[0044] 80 g of the polymerization product, 100 g of dichloromethane and 40 g of hexamethylenetetramine were mixed, the pH value of the system was adjusted to 9 with a NaOH solution, and then reacted at 50° C. for 12 h to obtain an aminated product.

[0045] 120 g of the amination product, 200 g of formaldehyde solution, 250 g of diisoamyl phosphite and 50 g of citric acid were mixed, reacted at 85° C. for 15 h, the solid was filtered out, and washed with water until neutral to obtain a uranium adsorption resin.

[0046] Comparative Example 2

[0047] The difference from Example 1 is that diethyl phosphite is replaced by phosphorous acid.

[0048] The adsorption performance of the adsorption resins of Example 1 and Comparative Examples 1-2 was tested in different acidic phosphorus-containing and uranium-containing wastewaters. The results are shown in Table 1.

[0049] Table 1

[0050]

[0051] As can be seen from the above table, the adsorption capacity of uranium by the uranium adsorption resin is above 40 mg / g, and can reach up to 61.6 mg / g. The uranium adsorption resin of the present invention has a good adsorption effect on uranium in acidic phosphorus-containing and uranium-containing wastewater.

[0052] When the concentration of phosphate is 3.22 g / L and the concentration of hydrogen ions is 0.2 mol / L, the equilibrium adsorption amount of uranium is 61.6 mg / g. When the concentration of hydrogen ions increases to 2.0 mol / L, the equilibrium adsorption amount of uranium can still reach 51.5 mg / g, indicating that the uranium adsorption resin of the present invention has good tolerance to acid.

[0053] When the hydrogen ion concentration is 1.0 mol / L and the phosphate concentration is 3.22 g / L (equivalent to a phosphorus content of 1.05 g / L), the equilibrium adsorption amount of uranium is 54.9 mg / g; when the phosphate concentration increases to 44.4 g / L (equivalent to a phosphorus content of 14.5 g / L), the equilibrium adsorption amount of uranium can still reach more than 40 mg / g, indicating that the uranium adsorption resin of the present invention has good tolerance to phosphorus.

[0054] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for preparing a uranium adsorption resin for adsorbing uranium in acidic phosphorus-containing and uranium-containing wastewater, It is characterized in that The following steps are involved: (1) 100 to 150 parts by weight of p-chlorostyrene, 9.5 to 15 parts by weight of divinylbenzene and 1.2 to 2.0 parts by weight of an initiator are mixed, and then mixed with 11 to 20 parts by weight of C5-C9 chain alkane to obtain an organic phase; the organic phase is mixed with 500 to 700 parts by weight of a dispersant solution, and reacted at 60 to 90° C. for 7 to 12 hours to obtain a polymer product; the C5-C9 chain alkane is a mixture of straight-chain alkanes and branched-chain alkanes, and the weight ratio of the straight-chain alkanes to the branched-chain alkanes in the mixture is 1:1 to 3; (2) swelling the polymer product, then adding 50 to 80 parts by weight of ethylenediamine, and reacting at 60 to 80° C. for 12 to 18 hours to obtain an aminated product; (3) mixing the amination product with 300 to 500 parts by weight of formaldehyde solution, 300 to 400 parts by weight of diethyl phosphite and 80 to 150 parts by weight of concentrated hydrochloric acid, and reacting at 80 to 95° C. for 12 to 24 hours to obtain a uranium adsorption resin; The hydrogen ion concentration in acidic phosphorus and uranium-containing wastewater is 0.2-2.0 mol / L, and the phosphate concentration is not higher than 45 g / L.

2. The preparation method according to claim 1, Features: The initiator is selected from one of benzoyl peroxide, azobisisobutyronitrile and lauroyl peroxide; The dispersant solution contains 0.1-1 wt% of a dispersant; the dispersant is selected from polyvinyl alcohol, oxidized polyvinyl alcohol, and polymaleic acid.

3. The preparation method according to claim 1, Features: The straight-chain alkane is selected from one or more of n-pentane, n-hexane, n-heptane and n-octane; The branched alkane is selected from one or more branched alkanes with methyl, dimethyl or trimethyl groups.

4. The uranium adsorption resin obtained by the preparation method according to any one of claims 1 to 3, It is characterized in that The uranium adsorption resin has an adsorption capacity of 40 mg / g or more for uranium.

5. Use of the uranium adsorption resin according to claim 4 in adsorbing uranium in acidic phosphorus-containing and uranium-containing wastewater.

Citation Information

Patent Citations

  • A sulfuric acid and chloride resistant uranium chelating resin and its synthesis method

    CN106507795B

  • Preparation method of uranium-adsorbing narrow-particle-size-distribution strong-basicity resin

    CN113501901A

  • Process for preparing heterodisperse chelating resins

    US20020185443A1