A method for preparing encapsulated bismuth vanadate powder
The preparation process of bismuth vanadate powder is simplified through spray drying envelope technology, and the problem of the darkening of bismuth vanadate pigment at high temperatures is solved, and process simplification, energy consumption reduction and product quality improvement are achieved.
Patent Information
- Application Number
- CN202211552577.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-05
AI Technical Summary
The existing bismuth vanadate pigments become darker or blacker when calcined above 600°C, and the process is complicated and the process flow is long, resulting in high cost and low efficiency.
The liquid mixed with bismuth vanadate powder and the envelope agent is used for spray-drying the envelope, and the encapsulated bismuth vanadate powder is formed by sonication and adjustment of pH, avoiding calcination, simplifying the process flow and reducing energy consumption.
The coating method with simple process, short process and low energy consumption is realized, which improves the uniformity, temperature resistance and fluidity of bismuth vanadate powder, reduces production costs, and avoids the generation of wastewater and waste gas.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional material preparation, and in particular relates to a coating method for bismuth vanadate pigment powder. Background Art
[0002] Bismuth vanadate (BiVO4) has excellent properties of being non-toxic, weather-resistant, bright in color and environmentally friendly, so it can be used to replace pigments containing toxic elements such as lead, cadmium, and chromium. It is a green and environmentally friendly inorganic yellow pigment with market prospects. However, the color of pure bismuth vanadate yellow pigment becomes darker or even black when calcined to above 600°C. Therefore, bismuth vanadate must be coated on the surface to form a high-temperature resistant coating on its surface.
[0003] Chinese Patent: CN104830099A discloses a method for preparing a coated silica-bismuth vanadate-barium sulfate high-brightness yellow pigment, wherein barium sulfate powder is mixed with a 0.2-0.6M bismuth vanadate precursor solution, ground for 20 minutes, and the mixture is taken out and dried at 50-80°C, and then ground for 20 minutes after drying. The ground powder is calcined at 400-500°C for 2-4 hours and then ball-milled for 12 hours to obtain a bismuth vanadate @ barium sulfate composite powder, which is then mixed with a 0.1-0.3M silica precursor solution and ground for 20 minutes, dried and ground for 20 minutes, calcined at 400-500°C for 2-4 hours and then ball-milled for 12 hours to prepare a coated silica @ bismuth vanadate @ barium sulfate pigment. Compared with the prior art, the present invention has only one layer of bismuth vanadate on the surface of barium sulfate, which greatly reduces the amount of expensive bismuth vanadate used, thereby reducing the cost of the yellow pigment; moreover, while reducing the cost, the color performance of the composite powder is still excellent, and its brightness and tinting power are better than those of pure bismuth vanadate, and has extremely high promotion and utilization value.
[0004] However, this patent has the defects of complex process and long process flow. Summary of the invention
[0005] In order to solve the above-mentioned technical problems existing in the prior art, the present invention provides a coating method for bismuth vanadate pigment powder. The present invention adopts a liquid obtained by mixing bismuth vanadate powder and a coating agent for spray drying and coating, which has the advantages of simple process, short process flow, no calcination process and low energy consumption.
[0006] The present invention is achieved through the following technical solutions:
[0007] The invention provides a method for preparing coated bismuth vanadate powder. A mixed liquid of bismuth vanadate powder and a coating agent is spray-dried in high-temperature air to obtain the coated bismuth vanadate powder.
[0008] Further, step A: taking bismuth vanadate powder to prepare bismuth vanadate powder dispersion;
[0009] Step B: preparing a coating agent solution by taking the coating agent, and adjusting the pH of the coating agent solution to prepare a coating agent sol;
[0010] Step C: adding the coating agent sol dropwise to the bismuth vanadate powder dispersion, stirring evenly, and adjusting the pH to obtain an encapsulated bismuth vanadate precursor;
[0011] Step D: adding the encapsulated bismuth vanadate precursor into a spray dryer, and performing spray drying in the spray dryer to obtain encapsulated bismuth vanadate powder.
[0012] Further, step A comprises the following steps:
[0013] A100: Take bismuth vanadate powder, add water and dispersant and stir;
[0014] A200: Ultrasonic treatment to obtain bismuth vanadate powder solution.
[0015] Furthermore, each liter of bismuth vanadate powder solution contains 0.5-1.0 mol of bismuth vanadate powder; and each liter of bismuth vanadate solution contains 0.01-0.1 mol of dispersant.
[0016] Furthermore, the dispersant is one of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide and polyethylene glycol.
[0017] Further, step B comprises the following steps:
[0018] B100: Take the coating agent and add water, stir and heat to prepare a coating agent solution with a concentration of 0.3-0.6 mol / L;
[0019] B200: Add 5-10% by volume sulfuric acid solution to the coating agent solution to adjust the pH value of the coating agent solution to 6-8, and stir at 70-90° C. for 1-3 hours to obtain a coating agent sol.
[0020] Furthermore, the coating agent is one of silicon-containing salt, aluminum-containing salt and titanium-containing salt.
[0021] Furthermore, in step C, the pH value is adjusted to 8-9.
[0022] Furthermore, the parameters of the spray dryer are controlled as follows: the feed rate of the encapsulated bismuth vanadate precursor is 0.6-1.2 L / h, the rotation speed of the centrifugal atomizer is ≥300 rpm, and the inlet air temperature is 120-200°C.
[0023] By adopting the above technical solution, the present invention has the following advantages:
[0024] 1. The present invention uses a liquid mixed with bismuth vanadate powder and a coating agent for spray drying and coating, which has the advantages of simple process, short process flow, no calcination process, and low energy consumption.
[0025] 2. The present invention uses a dispersant for ultrasonic pre-dispersion, which can effectively ensure the dispersibility of the bismuth vanadate powder. The subsequent spray drying can ensure the uniformity of the coating process, and the coating agent and the powder are more firmly combined under spraying and high temperature, thereby enhancing the temperature resistance of the powder.
[0026] 3. The present invention does not involve liquid-phase and solid-phase reactions, does not generate wastewater and waste, and does not pollute the environment.
[0027] 4. The coating method of the bismuth vanadate powder of the present invention is simple, efficient and easy to control, which solves the problems of complex process, poor controllability and low efficiency in the conventional powder coating process; the prepared coated bismuth vanadate powder has good uniformity, temperature resistance, fluidity and solubility, and the product quality is excellent.
[0028] 5. The overall process flow of the present invention is short, and there is no problem of wastewater and waste gas generated by both liquid and solid phase reactions and the process is difficult to control; the present invention places the encapsulated bismuth vanadate precursor in a spray dryer, controls the feed rate, the speed of the centrifugal atomizer, and the inlet air temperature, and performs spray drying and granulation to obtain encapsulated bismuth vanadate powder, which has the advantages of simple and controllable process, short process flow, no calcination process, and low energy consumption.
[0029] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and claims. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] This embodiment provides a method for preparing coated bismuth vanadate powder, wherein a mixed liquid of bismuth vanadate powder and a coating agent is spray-dried in high-temperature air to obtain the coated bismuth vanadate powder.
[0033] A method for preparing encapsulated bismuth vanadate powder can be specifically divided into the following steps:
[0034] Step A: preparing bismuth vanadate powder into a bismuth vanadate powder dispersion;
[0035] A100: take bismuth vanadate powder, add water and dispersant and stir; A200: ultrasonic treatment to obtain bismuth vanadate powder solution. Based on this, the dispersion effect and dispersion efficiency of bismuth vanadate powder can be improved.
[0036] Step B: preparing a coating agent solution by taking the coating agent, and adjusting the pH of the coating agent solution to prepare a coating agent sol;
[0037] B100: Take the coating agent and add water, stir and heat to prepare a coating agent solution with a concentration of 0.3-0.6 mol / L;
[0038] B200: add 5-10% sulfuric acid solution to the coating agent solution to adjust the pH value of the coating agent solution to 6-8, and stir at 70-90°C for 1-3h to obtain a coating agent sol. The coating agent sol thus obtained can better coat bismuth vanadate powder.
[0039] Step C: adding the coating agent sol dropwise to the bismuth vanadate powder dispersion, stirring evenly, and adjusting the pH to obtain an encapsulated bismuth vanadate precursor;
[0040] Step D: adding the encapsulated bismuth vanadate precursor into a spray dryer, and performing spray drying in the spray dryer to obtain encapsulated bismuth vanadate powder.
[0041] Furthermore, each liter of bismuth vanadate powder solution contains 0.5-1.0 mol of bismuth vanadate powder; each liter of bismuth vanadate solution contains 0.01-0.1 mol of dispersant. Based on this, the bismuth vanadate powder is dispersed without using too much dispersant, and the bismuth vanadate powder can also be guaranteed to have a better coating effect.
[0042] Furthermore, the dispersant is one of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, and polyethylene glycol. Of course, the dispersant is not limited to the above examples, and other dispersants in the prior art can also be applied to the present invention.
[0043] Furthermore, the coating agent is one of silicon-containing salt, aluminum-containing salt and titanium-containing salt.
[0044] Furthermore, in step C, the pH value is adjusted to 8-9.
[0045] Furthermore, the parameters of the spray dryer are controlled as follows: the feed rate of the encapsulated bismuth vanadate precursor is 0.6-1.2 L / h, the rotation speed of the centrifugal atomizer is ≥300 rpm, and the inlet air temperature is 120-200°C.
[0046] Example 2
[0047] This embodiment provides a method for preparing encapsulated bismuth vanadate powder.
[0048] Step A: preparing bismuth vanadate powder into a bismuth vanadate powder dispersion;
[0049] A100: Take bismuth vanadate powder, add water and dispersant and stir;
[0050] A200: Ultrasonic treatment is performed to obtain a bismuth vanadate powder solution. Each liter of the bismuth vanadate powder solution contains 0.5-1.0 mol of bismuth vanadate powder; each liter of the bismuth vanadate solution contains 0.01-0.1 mol of a dispersant.
[0051] Step B: preparing a coating agent solution by taking the coating agent, and adjusting the pH of the coating agent solution to prepare a coating agent sol;
[0052] B100: Take the coating agent and add water, stir and heat to prepare a coating agent solution with a concentration of 0.3-0.6 mol / L;
[0053] B200: add 5-10% sulfuric acid solution to the coating agent solution to adjust the pH value of the coating agent solution to 6-8, and stir at 70-90°C for 1-3h to obtain a coating agent sol. The coating agent sol thus obtained can better coat bismuth vanadate powder.
[0054] Step C: adding the coating agent sol dropwise to the bismuth vanadate powder dispersion, stirring evenly, and adjusting the pH value to 8-9 to obtain an encapsulated bismuth vanadate precursor;
[0055] Step D: adding the encapsulated bismuth vanadate precursor to a spray dryer, wherein the parameters of the spray dryer are controlled as follows: the feed rate of the encapsulated bismuth vanadate precursor is 0.6-1.2 L / h, the speed of the centrifugal atomizer is ≥300 rpm, and the inlet air temperature is 120-200° C.; the spray dryer performs spray drying to obtain encapsulated bismuth vanadate powder.
[0056] Furthermore, the dispersant is one of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, and polyethylene glycol. Of course, the dispersant is not limited to the above examples, and other dispersants in the prior art can also be applied to the present invention.
[0057] Furthermore, the coating agent is one of silicon-containing salt, aluminum-containing salt and titanium-containing salt.
[0058] Example 3
[0059] Take bismuth vanadate powder, add water and sodium dodecylbenzene sulfonate and stir evenly, then ultrasonically treat for 10 minutes to prepare a bismuth vanadate powder dispersion with a bismuth vanadate concentration of 0.5 mol / L and a sodium dodecylbenzene sulfonate concentration of 0.01 mol / L. Take a silicon-containing salt and prepare a solution with a concentration of 0.3 mol / L, add a 5% sulfuric acid solution by volume to adjust the pH of the coating agent solution to 6, and stir at 70°C for 1h to prepare a silicon-containing coating agent sol for standby use. Add the silicon-containing coating sol dropwise to the bismuth vanadate powder dispersion, stir evenly, adjust the pH to 8, and prepare a coated bismuth vanadate precursor. Add the coated bismuth vanadate precursor to a spray dryer, control the feed rate to 0.6 L / h, the centrifugal atomizer speed to 300 rpm, and the inlet air temperature to 120°C, and spray dry to obtain a coated bismuth vanadate powder.
[0060] Example 4
[0061] Take bismuth vanadate powder, add water and hexadecyl trimethyl ammonium bromide and stir evenly, then ultrasonically treat for 15 minutes to prepare a bismuth vanadate powder dispersion with a bismuth vanadate concentration of 1.0 mol / L and a hexadecyl trimethyl ammonium bromide concentration of 0.1 mol / L. Take an aluminum salt and prepare a solution with a concentration of 0.6 mol / L, add a 10% sulfuric acid solution by volume to adjust the pH of the coating agent solution to 8, and stir at 90°C for 3 hours to prepare an aluminum-containing coating agent sol for standby use. Add the aluminum-containing coating sol dropwise to the bismuth vanadate powder dispersion, stir evenly, adjust the pH to 9, and prepare a coated bismuth vanadate precursor. Add the coated bismuth vanadate precursor to a spray dryer, control the feed rate to 1.2 L / h, the centrifugal atomizer speed to 300 rpm, and the inlet air temperature to 200°C, and spray dry to obtain a coated bismuth vanadate powder.
[0062] Example 5
[0063] Take bismuth vanadate powder, add water and sodium dodecylbenzene sulfonate and stir evenly, then ultrasonically treat for 10 minutes to prepare a bismuth vanadate powder dispersion with a bismuth vanadate concentration of 0.5 mol / L and a sodium dodecylbenzene sulfonate concentration of 0.05 mol / L. Take a silicon-containing salt and prepare a solution with a concentration of 0.5 mol / L, add a 5% sulfuric acid solution by volume to adjust the pH of the coating agent solution to 8, and stir at 90°C for 2 hours to prepare a silicon-containing coating agent sol for standby use. Add the silicon-containing coating sol dropwise to the bismuth vanadate powder dispersion, stir evenly, adjust the pH to 8, and prepare a coated bismuth vanadate precursor. Add the coated bismuth vanadate precursor to a spray dryer, control the feed rate to 0.6 L / h, the centrifugal atomizer speed to 500 rpm, and the inlet air temperature to 150°C, and spray dry to obtain the coated bismuth vanadate powder.
[0064] Example 6
[0065] Take bismuth vanadate powder, add water and hexadecyl trimethyl ammonium bromide and stir evenly, then ultrasonically treat for 15 minutes to prepare a bismuth vanadate powder dispersion with a bismuth vanadate concentration of 1.0 mol / L and a hexadecyl trimethyl ammonium bromide concentration of 0.1 mol / L. Take an aluminum salt and prepare a solution with a concentration of 0.6 mol / L, add a 10% sulfuric acid solution by volume to adjust the pH of the coating agent solution to 7, and stir at 80°C for 3 hours to prepare an aluminum coating agent sol for standby use. Add the aluminum coating sol dropwise to the bismuth vanadate powder dispersion, stir evenly, adjust the pH to 9, and prepare a coated bismuth vanadate precursor. Add the coated bismuth vanadate precursor to a spray dryer, control the feed rate to 1.0 L / h, the centrifugal atomizer speed to 300 rpm, and the inlet air temperature to 200°C, and spray dry to obtain a coated bismuth vanadate powder.
[0066] Example 7
[0067] Take bismuth vanadate powder, add water and polyethylene glycol and stir evenly, ultrasonically treat for 12 minutes, and prepare a bismuth vanadate powder dispersion with a bismuth vanadate concentration of 0.8 mol / L and a polyethylene glycol concentration of 0.01 mol / L. Take a titanium salt and prepare a solution with a concentration of 0.3 mol / L, add a sulfuric acid solution with a volume fraction of 8% to adjust the pH of the coating agent solution to 6, and stir at 70°C for 1h to prepare a titanium-containing coating agent sol for standby use. Add the titanium-containing coating sol dropwise to the bismuth vanadate powder dispersion, stir evenly, adjust the pH to 8, and prepare a coated bismuth vanadate precursor. Add the coated bismuth vanadate precursor to a spray dryer, control the feed rate to 1.2 L / h, the centrifugal atomizer speed to 800 rpm, and the inlet air temperature to 120°C, and spray dry to obtain a coated bismuth vanadate powder.
[0068] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing encapsulated bismuth vanadate powder, It is characterized in that The mixed liquid of bismuth vanadate powder and coating agent is spray-dried in high temperature air to obtain coated bismuth vanadate powder; Step A: A100: Take bismuth vanadate powder, add water and dispersant and stir; A200: ultrasonic treatment to obtain bismuth vanadate powder dispersion; Step B: B100: Take the coating agent and add water, stir and heat to prepare a coating agent solution with a concentration of 0.3-0.6 mol / L; B200: adding 5-10% by volume sulfuric acid solution to the coating agent solution to adjust the pH value of the coating agent solution to 6-8, stirring at 70-90° C. for 1-3 hours to obtain a coating agent sol; Step C: adding the coating agent sol dropwise to the bismuth vanadate powder dispersion, stirring evenly, and adjusting the pH to obtain an encapsulated bismuth vanadate precursor; Step D: adding the encapsulated bismuth vanadate precursor into a spray dryer, and performing spray drying in the spray dryer to obtain encapsulated bismuth vanadate powder.
2. A method for preparing a coated bismuth vanadate powder as claimed in claim 1, It is characterized in that Each liter of bismuth vanadate powder dispersion contains 0.5-1.0 mol of bismuth vanadate powder; each liter of bismuth vanadate powder dispersion contains 0.01-0.1 mol of dispersant.
3. A method for preparing a coated bismuth vanadate powder as claimed in claim 1, It is characterized in that The dispersant is one of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide and polyethylene glycol.
4. A method for preparing a coated bismuth vanadate powder as claimed in claim 1, It is characterized in that The coating agent is one of silicon-containing salt, aluminum-containing salt and titanium-containing salt.
5. A method for preparing an encapsulated bismuth vanadate powder as claimed in claim 1, It is characterized in that In the step C, the pH value is adjusted to 8-9.
6. A method for preparing an encapsulated bismuth vanadate powder as claimed in claim 1, It is characterized in that The parameters of the spray dryer are controlled as follows: the feed rate of the encapsulated bismuth vanadate precursor is 0.6-1.2 L / h, the rotation speed of the centrifugal atomizer is ≥300 rpm, and the inlet air temperature is 120-200°C.