A method for preparing a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head

Through the pretreatment of nano-carbon nanotubes and silicon carbide, ball milling and electromagnetic stirring and smelting processes, carbon nanotube-silicon carbide-aluminum composite materials are formed, which solves the problem of low strength of the insulated operating rod working head and significantly improves mechanical strength and extension Rate to meet the needs of lightweight and high strength.

CN116179885BActive Publication Date: 2024-11-05HUZHOU ELECTRIC POWER SUPPLY CO OF STATE GRID ZHEJIANG ELECTRIC POWER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310061950.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-11-05
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

The strength of the existing insulated operating rod working head is low, making it difficult to meet the needs of lightweight and high strength, especially when used in high-voltage transmission lines, the problems of bending and unstable grip are prone to occur.

Method used

The pretreatment of nanocarbon nanotubes and silicon carbide is made of carbon nanotubes-silicon carbide-aluminum composite material, and ball milling, electromagnetic stirring and calcining casting processes are adopted, which significantly improves the mechanical strength of the material.

Benefits of technology

The mechanical strength and elongation of the insulated operating rod working head are significantly improved, the dispersion of the material and the interface bonding strength are enhanced, and the problem of insufficient strength in the prior art is solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116179885B_ABST
    Figure CN116179885B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ultra-high voltage electrical equipment, and discloses a method for preparing a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head. The method comprises the following steps: (1) heat-treating carbon nanotubes to prepare heat-treated carbon nanotubes, and acid-treating the heat-treated carbon nanotubes to prepare purified carbon nanotubes; (2) roasting quartz sand and coke to prepare a crude silicon carbide product, and then purifying the crude silicon carbide product to prepare purified silicon carbide; (3) ball-milling the purified carbon nanotubes, the purified silicon carbide and aluminum powder to prepare a carbon nanotube-silicon carbide-aluminum composite material; (4) subjecting the carbon nanotube-silicon carbide-aluminum composite material to electromagnetic stirring smelting treatment to prepare a carbon-silicon-aluminum alloy; and (5) forging the carbon-silicon-aluminum alloy to prepare a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head. The method has simple process, simple equipment, low cost and significantly improves the mechanical strength of the insulating operating rod working head.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ultra-high voltage electrical equipment, and in particular to a method for preparing a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head. Background Art

[0002] The insulating operating rod consists of three parts: the working head, the insulating rod and the handle. The working head is at the front end of the operating rod during installation, and its weight has a great influence on the user's feel. If the operating head is heavy, the operating rod is prone to bending and unstable during use. Therefore, lightweight is an important indicator in the preparation process of the insulating operating rod working head. In addition, since the operating rod often plays a supporting and connecting role during use, high strength is also an important indicator in the preparation process of the insulating operating rod working head.

[0003] In order to meet the requirements of light weight and high strength, the working head in the prior art is generally cast from 6 series aluminum alloy. 6 series aluminum alloy is an Al-Mg-Si series aluminum alloy that can be heat-treated and strengthened. The mass fraction of Mg2Si is generally 0.8-1.2%. This type of alloy has a high solid solution treatment temperature, low quenching sensitivity, and very good formability. It can be quenched online on a press. Although 6 series aluminum alloy has lightweight performance, its impact and tensile strength are medium. At present, carbon silicon aluminum alloys made of silicon carbide particles and aluminum have gradually improved strength on the basis of lightweight performance. For example, the tensile strength of SiCp / 2024Al composite materials can be increased by 20%, and it also has good high temperature stability. For example, 15% SiC / 2009 composite materials and 25% SiC / 6092 have high strength and high toughness. However, the material strength of the above aluminum alloy materials needs to be improved. Summary of the invention

[0004] In order to overcome the problem of low strength of the working head made by the preparation process of the insulating operating rod working head in the prior art, a method for preparing a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head is provided. This method pretreats carbon nanotubes and silicon carbide so that the carbon nanotube and silicon carbide mixed reinforced particles can be fully dispersed in the aluminum matrix, and then a lightweight and high-strength aluminum alloy high-voltage transmission line insulating operating rod working head is made through a specific ball milling process, a smelting and refining process, and a forging and casting process. The mechanical strength of the product made by this process is significantly improved.

[0005] The specific technical scheme of the present invention is:

[0006] A method for preparing a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head comprises the following steps:

[0007] (1) heat-treating the carbon nanotubes to obtain heat-treated carbon nanotubes, and acid-treating the heat-treated carbon nanotubes to obtain purified carbon nanotubes;

[0008] (2) roasting quartz sand and coke to produce crude silicon carbide, and then purifying the crude silicon carbide to produce purified silicon carbide, wherein the purification process includes high-temperature oxidation treatment;

[0009] (3) ball-milling the purified carbon nanotubes, purified silicon carbide and aluminum powder to prepare a carbon nanotube-silicon carbide-aluminum composite material; (4) subjecting the carbon nanotube-silicon carbide-aluminum composite material to electromagnetic stirring melting to prepare a carbon-silicon-aluminum alloy;

[0010] (5) Forging carbon-silicon-aluminum alloy into a lightweight, high-strength aluminum alloy ultra-high voltage transmission line insulation operating rod working head

[0011] The present application provides a method for preparing a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head, which method sequentially comprises five steps: nano carbon nanotube purification, silicon carbide purification, carbon nanotube-silicon carbide-aluminum composite material preparation, electromagnetic stirring melting treatment and forging process.

[0012] The purpose of purifying nano carbon nanotubes is to remove catalyst particles, other forms of impurity carbon, and structural defects in the growth process of carbon nanotubes. Amorphous carbon in carbon nanotubes can be removed by heat treatment, and metal catalyst impurities can be removed by acid treatment. After purifying nano carbon nanotubes, the agglomeration phenomenon between carbon nanotubes can be effectively improved, and the dispersion of carbon nanotubes can be significantly improved.

[0013] The purpose of silicon carbide purification is to remove free carbon and free impurities (iron oxide, silicon, quartz sand, Fe, Mn, Ni, V) in crude silicon carbide. Carbon impurities will form brittle phase Al in aluminum alloy. 4 C 3 , brittle phase Al 4 C 3 It will lead to a decrease in the strength of the alloy. Therefore, it is necessary to control the Al content in the aluminum alloy. 4 C 3 The content has an important influence on improving the strength of aluminum alloy.

[0014] The preparation of carbon nanotube-silicon carbide-aluminum composite material adopts ball milling. Under the repeated impact of ball milling media, carbon nanotubes, silicon carbide and aluminum powder are subjected to the combined effects of impact, shear, friction and compression, and have undergone repeated extrusion, cold welding and crushing. During this process, purified carbon nanotubes and purified silicon carbide are dispersed on the surface of aluminum powder or embedded in the welded aluminum powder. For aluminum alloy matrix, high-energy ball milling disperses carbon nanotubes while mechanical alloying occurs between the powders of various elements, eventually forming carbon nanotube-silicon carbide-aluminum composite material.

[0015] The present application uses an electromagnetic stirring melting process with simple process, simple equipment and low cost, and determines the optimal electromagnetic stirring conditions and melting and refining conditions. During the melting process, the aluminum alloy matrix and the carbon nanotube-silicon carbide reinforcement have an important influence on the synthesis of the carbon-silicon-aluminum alloy under the electromagnetic stirring conditions and melting and refining conditions. When the temperature is low, the wetting angle between the aluminum alloy liquid and the carbon nanotube-silicon carbide reinforcement is large, and the bonding force between the two is insufficient, resulting in the final carbon-silicon-aluminum alloy. The strength is low, and the high temperature is easy to generate brittle phase Al 4 C 3 , brittle phase Al 4 C 3 The accumulation of carbon nanotubes and silicon carbide reinforcements will lead to deterioration of the performance of the composite material. The stirring time has a great influence on the dispersibility of carbon nanotube-silicon carbide reinforcements in the aluminum alloy liquid. When the time is short, the dispersion state in the solid solution phase is poor and there are more agglomerates. When the stirring time is too long, the dispersion is not significantly improved. In addition, the volume fraction of carbon nanotube-silicon carbide reinforcements also has a great influence on their dispersibility in the aluminum matrix. If the volume fraction of carbon nanotube-silicon carbide reinforcements is too large, it will lead to uneven dispersion, and if it is too small, it will cause particles to agglomerate.

[0016] The forging process in the present application adopts a hot forging process, which significantly improves the tensile strength and elongation of the carbon silicon aluminum alloy. The main reasons for the above improvement are: improving the uniformity of the distribution of carbon nanotube-silicon carbide mixed particles, and improving the interface bonding strength between the carbon nanotube-silicon carbide mixed reinforced particles and the aluminum matrix. There is obvious particle aggregation in the cast composite material, so it is easy to break during the stretching process, and the strength and elongation are very low. The distribution of carbon nanotube-silicon carbide mixed reinforced particles in the carbon silicon aluminum material after hot forging will be more uniform. In addition, the strengthening of the particle reinforced composite material mainly depends on the transfer of load from the matrix to the reinforcement particles. The particles are the main load carriers, and the load transfer is completed through the interface between the two. The interface bonding strength between the carbon nanotube-silicon carbide mixed reinforced particles and the aluminum matrix is ​​improved, which helps to improve the reinforcing effect of the carbon nanotube-silicon carbide reinforcement on the strength and elongation strength of the carbon silicon aluminum alloy.

[0017] The amount of deformation and heating conditions during hot forging play an important role in the performance of the material. Under different temperatures and different deformation conditions, the grain morphology inside the carbon-silicon-aluminum alloy will be different. When deformation occurs, the grains will be elongated, broken, and form sub-grains. Too high a deformation temperature will induce recrystallization of the alloy, which is not conducive to maintaining the deformed structure and affects the performance of the alloy. If the deformation temperature exceeds the overburning point of the alloy, the structure of the alloy will be destroyed, and the plasticity and mechanical properties of the alloy will be significantly reduced. If the temperature is too low, the plasticity of the alloy is poor, and effective deformation cannot occur, resulting in fracture.

[0018] Preferably, the carbon nanotubes in step (1) are multi-walled carbon nanotubes, the carbon nanotubes are 5 to 15 μm long and the tube diameter is 20 to 30 nm; the nano carbon nanotubes in the present application are selected from long and thin shapes with a large aspect ratio. Generally, the aspect ratio of carbon nanotubes has a great influence on their dispersibility. Short and thick carbon nanotubes with a small aspect ratio have high dispersibility, but their improvement on the performance of the alloy is not significant. Although long and thin carbon nanotubes with a large aspect ratio can significantly improve the performance of the alloy, their dispersion performance is low. The nano carbon nanotubes of the present application can significantly show high dispersibility and effective cross-sectional bonding in the alloy after pretreatment and ball milling.

[0019] Preferably, the high-temperature oxidation treatment conditions in step (2) are: a temperature of 700-900°C and a holding time of 3-10 hours, and the purification treatment also includes ultrasonic cleaning, water washing, drying and screening; the high-temperature oxidation treatment in the present application is obtained through strict experimental screening. If the oxidation temperature is too low, the oxidation rate and the thickness of the oxide layer will be insufficient, and the loose state of the final product material will account for a significantly higher proportion than the aggregated state, and the particle structure is prone to looseness. If the temperature is too high, the oxidation rate of the final product will not increase significantly, and the particles will sinter, affecting the particle quality.

[0020] Preferably, the ball milling treatment conditions in step (3) are: the ball milling time is 3 to 12 hours.

[0021] Preferably, the total reinforcement content of carbon nanotubes-silicon carbide in the carbon nanotube-silicon carbide-aluminum composite material in step (3) is 2-15%.

[0022] Preferably, the particle size of silicon carbide in the carbon nanotube-silicon carbide-aluminum composite material in step (4) is 15 to 300 μm.

[0023] Preferably, the electromagnetic stirring melting treatment in step (4) includes initial melting treatment and electromagnetic stirring melting treatment in sequence.

[0024] Preferably, the initial melting conditions are: placing the carbon nanotube-silicon carbide-aluminum composite material in a 710°C crucible and then heating it to 720°C to melt, removing slag after melting and cooling it to 710°C for 5 minutes, and then treating it with hexachloroethane for 10 minutes.

[0025] Preferably, the electromagnetic stirring melting conditions are: electromagnetic stirring frequency is 6 Hz, current intensity is 450 A, stirring temperature is 690-710° C., and melting time is greater than 60 min.

[0026] Preferably, the forging conditions in step (5) include initial forging, tempering and final forging in sequence, the initial forging temperature is 430°C, the final forging condition is 380°C, and the forging deformation of the carbon-silicon-aluminum alloy is 40-60%.

[0027] Compared with the prior art, this application has the following technical effects:

[0028] (1) The preparation method provided by the present application has simple process, simple equipment and low cost;

[0029] (2) In the preparation method provided in the present application, the mechanical strength of the carbon silicon aluminum alloy is enhanced by using carbon nanotube-silicon carbide reinforcement. By optimizing the process conditions of the carbon nanotube purification process, the silicon carbide purification process, the carbon nanotube-silicon carbide-aluminum composite material preparation process, the electromagnetic stirring melting treatment and the forging process, the carbon nanotubes, silicon carbide and aluminum matrix are combined to form a carbon silicon aluminum alloy with significantly improved mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 These are scanning electron microscope images of the unpurified carbon nanotubes and purified carbon nanotubes of the present invention.

[0031] Figure 2 This is a scanning electron microscope image of silicon carbide of the present invention at an oxidation temperature of 800° C. and a holding time of 8 hours.

[0032] Figure 3 The following are scanning electron microscope images of the carbon nanotube-silicon carbide-aluminum composites of the present invention at different ball milling times.

[0033] Figure 4 It is the tensile curve of the carbon-silicon-aluminum alloy with different silicon carbide particle sizes of the present invention.

[0034] Figure 5 1 is a scanning electron microscope image of the carbon-silicon-aluminum alloy forging casting at different deformation amounts / forging temperatures of the present invention. DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with the embodiments.

[0036] Embodiment 1:

[0037] A method for preparing a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head comprises the following steps:

[0038] (1) heat-treating carbon nanotubes to obtain heat-treated carbon nanotubes, and acid-treating the heat-treated carbon nanotubes to obtain purified carbon nanotubes, wherein the carbon nanotubes are multi-walled carbon nanotubes;

[0039] (2) roasting quartz sand and coke to obtain a crude silicon carbide product, and subjecting the crude silicon carbide product to ultrasonic cleaning, water washing, drying, high-temperature oxidation treatment, and screening in sequence to obtain purified silicon carbide;

[0040] (3) ball-milling the purified carbon nanotubes, purified silicon carbide and aluminum powder to prepare a carbon nanotube-silicon carbide-aluminum composite material;

[0041] (4) subjecting the carbon nanotube-silicon carbide-aluminum composite material to electromagnetic stirring melting treatment to prepare carbon silicon aluminum alloy; the electromagnetic stirring melting treatment includes initial melting treatment and electromagnetic stirring melting treatment in sequence; the initial melting conditions are: placing the carbon nanotube-silicon carbide-aluminum composite material in a 710°C crucible and then heating it to 720°C to melt, removing slag after melting and cooling it to 710°C for 5 minutes, and then treating it with hexachloroethane for 10 minutes; the electromagnetic stirring melting conditions are: electromagnetic stirring frequency of 6 Hz, current intensity of 450A, stirring temperature of 690°C, and melting time of 60 minutes;

[0042] (5) The carbon-silicon-aluminum alloy is forged and cast into a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head. The forging conditions include initial forging, tempering and final forging in sequence. The initial forging temperature is 430°C, the final forging condition is 380°C, and the forging deformation of the carbon-silicon-aluminum alloy is 40%.

[0043] Example 2: (Effect of high temperature oxidation treatment temperature)

[0044] The method of Example 1 was adopted, and the oxidation temperatures in step (2) were 700°C, 800°C and 900°C respectively. The other conditions were the same as those of Example 1, and the total mass before and after oxidation was detected. The results are shown in Table 1.

[0045] Table 1 Quality of silicon carbide after high temperature oxidation treatment at different temperatures

[0046]

[0047] As shown in the results in Table 1, when the oxidation temperature is 700°C and the temperature is kept warm for 10 hours, the oxidation rate of silicon carbide particles is 1.25%; when the oxidation temperature is 800°C and the temperature is kept warm for 10 hours, the oxidation rate of silicon carbide particles is 5.65%; when the oxidation temperature is 900°C and the temperature is kept warm for 10 hours, the oxidation rate of silicon carbide particles is 13.25%. Under the condition of 700℃ oxidation temperature and 10 hours of heat preservation, the total mass of silicon carbide particles before and after oxidation only increased by 0.0001g, and the oxidation percentage was 1.25%; under the condition of 800℃ oxidation temperature and 10 hours of heat preservation, the total mass of silicon carbide particles before and after oxidation increased by 0.0007g, and the oxidation percentage was 5.65%; under the condition of 900℃ oxidation temperature and 10 hours of heat preservation, the total mass of silicon carbide particles before and after oxidation increased by 0.0019g, and the oxidation percentage was 13.25%; By comparing the data and the calculation results, it can be concluded that the oxidation rate under the condition of 700℃ oxidation temperature and 10 hours of heat preservation is obviously too low, and the increase in the thickness of the oxide layer is extremely small, so the oxidation efficiency of silicon carbide is not high under this parameter condition;

[0048] Figure 2 This is a scanning electron microscope image with an oxidation temperature of 800°C and a holding time of 8h. Figure 2 As shown in the figure, the particles obtained by long-term high-temperature oxidation treatment have removed the sharp corners of the edge, indicating that the high-temperature oxidation treatment has a passivation effect. At the same time, as the reaction increases, the sharp corner passivation effect becomes more obvious. After 6 hours of oxidation at a temperature of 800°C, a layer of SiO2 will form on the surface of the silicon carbide particles, and the appearance of the nano-scale particles adsorbed on the surface will become smoother, and the interface with the silicon carbide particles will become more blurred. In addition, the energy at the smooth part is much lower than the energy at the sharp corner, so oxidation always starts at the surface of the nano-scale particles adsorbed on the particle surface or at the sharp corner of the particle;

[0049] In summary, the oxidation effect of silicon carbide powder particles is best when the temperature is 800℃ and the temperature is kept for 8h.

[0050] Example 3: (Effect of different ball milling times)

[0051] The method of Example 1 was adopted, and the ball milling time in step (3) was 3h, 5h, 7h and 9h respectively. The other conditions were the same as those in Example 1. The formed carbon nano-silicon carbide-aluminum composite material was subjected to scanning electron microscopy. The results are shown in FIG. Figure 3 ;

[0052] like Figure 3As shown in the figure, after 3 hours of mechanical ball milling, the spherical aluminum alloy particles are plastically deformed into flakes after impact, and there are more carbon nanotubes on the surface of the enlarged flake aluminum alloy; as the ball milling process proceeds (ball milling time 5 hours), the flake aluminum alloys are superimposed on each other and welded together to become irregular particles, and the carbon nanotubes are peeled off and embedded in the aluminum alloy particles; when the ball milling time is further extended to 7 hours and 9 hours, the powder agglomerates and coarsens, and the aluminum alloy particle size shows a trend of growing. At this time, the carbon nanotubes are basically invisible, indicating that the carbon nanotubes are completely embedded in the irregular spherical aluminum alloy powder.

[0053] Example 4: (Effect of different silicon carbide particle sizes)

[0054] The method of Example 1 is adopted, the particle size ranges of silicon carbide in the carbon nano-silicon carbide-aluminum composite material in step (4) are 15-55 μm, 100-150 μm and 200-300 μm respectively, and the other conditions are the same as those in Example 1. The tensile strength test and elongation test of the finally obtained carbon silicon aluminum alloy are performed, and the test results are shown in Table 2;

[0055] Table 2 Tensile strength and elongation after fracture of carbon-silicon-aluminum alloys with different silicon carbide particle sizes

[0056] Silicon carbide particle size Tensile strength(MPa) Elongation after break (%) 15~55μm 506(±14) 8.4(±0.5) 100~150μm 556(±18) 6.5(±0.5) 200~300μm 522(±16) 8.2(±0.5)

[0057] As shown in Table 2 and Figure 4 As shown in the figure, the SiC reinforced aluminum matrix composite material (Sample-2) with a particle size of 100-150μm has the best tensile strength, reaching 556MPa, which is about 50 and 34Mpa higher than the tensile strength of the SiC reinforced aluminum matrix composite material with a particle size of 15-55μm and 200-300μm, respectively. A high density of thermal mismatch density is generated in the matrix adjacent to the SiC particles of the composite material. It can be inferred that the generation of dislocations is mainly due to the thermal mismatch stress between the SiC particles and the matrix, and the appropriate particle size effectively releases the stress in the matrix near the SiC particles, greatly reducing the density of dislocations in the matrix due to the thermal mismatch stress between the matrix and SiC.

[0058] Example 5: (Effect of different carbon nanotube contents)

[0059] The method of Example 1 was adopted, and the contents of carbon nanotubes in the carbon nano-silicon carbide-aluminum composite material in step (4) were 5%, 10% and 15% respectively, and the other conditions were the same as those in Example 1. The yield strength, tensile strength and elongation tests of the finally obtained carbon silicon aluminum alloy were performed. The test results are shown in Tables 3 and Figure 4 ;

[0060] Table 3 Yield strength, tensile strength and elongation after fracture of carbon-silicon alloys with different carbon nanotube contents

[0061] Carbon nanotube content (%) Yield Strength(MPA) Tensile strength(MPa) Elongation after break (%) 0 281 307 14 5 417 468 9.5 10 506 529 7.5 15 461 488 3.6

[0062] As shown in Table 3, the yield strength, tensile strength and elongation of the carbon-silicon-aluminum alloy without carbon nanotubes are 281MPa, 307MPa and 14% respectively; the yield strength, tensile strength and elongation of the carbon-silicon-aluminum alloy sample with a carbon nanotube content of 5% are 417MPa, 468MPa and 9.5% respectively, which are 48% and 52% higher than the yield strength and tensile strength of the carbon-silicon-aluminum alloy without carbon nanotubes; the yield strength and tensile strength of the carbon-silicon-aluminum alloy sample with a carbon nanotube content of 10% are 417MPa, 468MPa and 9.5% respectively. The yield strength, tensile strength and elongation are 506MPa, 529MPa and 7.5% respectively, which are 80% and 72% higher than the yield strength and tensile strength of the carbon silicon aluminum alloy without carbon nanotubes; the yield strength, tensile strength and elongation of the carbon silicon aluminum alloy sample with 15% carbon nanotubes are 461MPa, 488MPa and 3.6% respectively, which are 64% and 59% higher than the yield strength and tensile strength of the carbon silicon aluminum alloy without carbon nanotubes. The results show that the yield strength and tensile strength of carbon nanotube-silicon carbide of carbon silicon aluminum alloy are the best when the carbon nanotube content is 10%; the elongation of the composite material is greatly reduced while the strength is improved; with the increase of carbon nanotube content, due to the inconsistency of the deformation ability of carbon nanotubes and aluminum matrix, carbon nanotube-silicon carbide strongly hinders the plastic deformation of aluminum matrix, resulting in cracking of the composite material at the weak interface, thereby reducing the elongation of the composite material.

[0063] Example 6 (Effect of forging temperature and deformation amount)

[0064] The method of Example 1 is adopted, and the deformation amount / forging temperature of the carbon-silicon-aluminum alloy in step (5) is set to 30% / 300°C, 50% / 300°C, 50% / 350°C, 50% / 420°C, 50% / 450°C and 50% / 500°C respectively; the other conditions are the same as those in Example 1, and the carbon-silicon-aluminum alloy forging after forging is scanned by electron microscope, and the results are shown as follows Figure 5 ;

[0065] from Figure 5It can be seen that when the deformation temperature is 300℃, due to the low temperature, the flow stress of the alloy is large, so cracks appear when the deformation is 40%, and the plasticity of the alloy is very poor at this time; after the alloy is deformed at 450℃, although the grain shape is still elongated fiber, the size increases; at 500℃, the grain size increases more significantly. Such a structure is not good for the strength of the alloy, so the optimal deformation temperature of the alloy should be lower than 450℃. In the subsequent forging process of the insulating operating rod end workpiece, we should use 450℃ as the upper limit of the forging temperature for process selection. The ultimate deformation and metallographic structure of the alloy at different deformation temperatures show that the optimal deformation temperature of the alloy is 400℃-420℃; when deformed at this temperature, the silicon carbide reinforced aluminum-based composite material can not only obtain better deformation performance, but also effectively prevent grain growth or recrystallization during the deformation process; considering that the heat loss during the die forging of the end forging of the insulating operating rod is relatively large, the initial forging temperature and final forging temperature of the carbon-silicon aluminum alloy are determined to be 430℃ and 380℃ respectively, and tempering is performed once during the forging process, which reduces the forging difficulty of the silicon carbide reinforced aluminum-based composite material, which is higher than that of conventional aluminum alloys, and makes the forging process more convenient.

[0066] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head, characterized in that: The following steps are involved: (1) heat-treating the carbon nanotubes to obtain heat-treated carbon nanotubes, and acid-treating the heat-treated carbon nanotubes to obtain purified carbon nanotubes; (2) roasting quartz sand and coke to produce crude silicon carbide, and then purifying the crude silicon carbide to produce purified silicon carbide, wherein the purification process includes high-temperature oxidation treatment, ultrasonic cleaning, water washing, drying and screening, and the conditions of the high-temperature oxidation treatment include: temperature of 800° C. and holding time of 8 hours; (3) ball-milling the purified carbon nanotubes, purified silicon carbide and aluminum powder to prepare a carbon nanotube-silicon carbide-aluminum composite material, wherein the ball-milling time is 7 to 9 hours, and the particle size of silicon carbide in the carbon nanotube-silicon carbide-aluminum composite material is 100 to 150 μm; (4) subjecting the carbon nanotube-silicon carbide-aluminum composite material to electromagnetic stirring melting treatment to prepare a carbon silicon aluminum alloy, wherein the carbon nanotube content in the carbon silicon aluminum alloy is 10%, and the electromagnetic stirring melting conditions are: electromagnetic stirring frequency of 6 Hz, current intensity of 450 A, stirring temperature of 690° C., and melting time of 60 min; (5) Forging a carbon-silicon-aluminum alloy into a lightweight, high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head; the forging conditions include initial forging, tempering and final forging in sequence, the initial forging temperature is 430° C., the final forging condition is 380° C., and the forging deformation of the carbon-silicon-aluminum alloy is 40-60%.

2. The preparation method according to claim 1, characterized in that: The carbon nanotubes described in step (1) are multi-walled carbon nanotubes.

3. The method for preparing a lightweight and high-strength aluminum alloy ultra-high voltage transmission line insulating operating rod working head according to claim 1, characterized in that: The carbon nanotubes described in step (1) are 5 to 15 μm long.

4. The preparation method according to claim 1, characterized in that: The diameter of the carbon nanotubes in step (1) is 20-30 nm.

5. The preparation method according to claim 1, characterized in that: The electromagnetic stirring melting treatment in step (4) includes initial melting treatment and electromagnetic stirring melting treatment in sequence.

6. The preparation method according to claim 5, characterized in that: The conditions of the initial melting treatment are: placing the carbon nanotube-silicon carbide-aluminum composite material in a 710° C. crucible and heating it to 720° C. to melt it, removing slag after melting and cooling it to 710° C. to keep it warm for 5 minutes, and then treating it with hexachloroethane for 10 minutes.

7. The preparation method according to claim 5, characterized in that: The conditions for the electromagnetic stirring melting treatment include: the electromagnetic stirring frequency is 6 Hz.

8. The preparation method according to claim 5, characterized in that: The conditions of the electromagnetic stirring melting treatment include: the current intensity is 450A.

9. The preparation method according to claim 5, characterized in that: The conditions of the electromagnetic stirring melting treatment include: the stirring temperature is 690-710°C.

10. The preparation method according to claim 5, characterized in that: The conditions for the electromagnetic stirring melting treatment include: the melting time is greater than 60 minutes.