A catalyst for preparing spiral nanocarbon fibers and its application
By using soluble LixCoy carbonate catalysts prepared by LiCl, CoCl2 and citric acid, the problems of high production costs of spiral nanocarbon fibers and easy catalyst agglomeration are solved, and efficient and low-cost preparation of spiral nanocarbon fibers and high-value reduction of waste tires are achieved. use.
Patent Information
- Application Number
- CN202310211542.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-07
AI Technical Summary
In the prior art, the mass production cost of spiral nanocarbon fibers is high and the catalysts are prone to agglomeration, which limits its industrial application.
LiCl, CoCl2 and citric acid are used as raw materials to prepare soluble LixCoy carbonate catalysts, and the catalyst residues are removed by simple water washing, reducing production costs and improving catalytic efficiency.
The efficient preparation of spiral nanocarbon fibers is achieved, the processing cost is reduced, the subsequent process is simplified, and the utilization value of waste tires and the yield of spiral nanocarbon fibers is improved.
Smart Images

Figure BDA0004112875150000031 
Figure BDA0004112875150000041 
Figure BDA0004112875150000042
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon nanofibers, and in particular to a catalyst for preparing helical carbon nanofibers and application thereof. Background Art
[0002] Due to its unique spiral structure, spiral carbon nanofibers have excellent conductivity, thermal stability, chemical stability and other properties, and have broad application prospects in gas storage, energy storage, microwave absorption and other fields.
[0003] At present, chemical vapor deposition is generally used to prepare spiral nanocarbon fibers. Usually, acetylene or ethylene carbon sources, nano Fe, Co, Ni, Cu and their nano alloy particles are used as catalysts, and spiral nanocarbon fibers are prepared by chemical vapor deposition at 500-700 ° C. The existing technology has considered using waste tires as a carbon source to prepare nanocarbon fibers. Because more than 1 billion waste tires are produced every year in the world, the recycling and reuse of waste tires has always been one of the issues of concern in the industry. There are a large number of waste tires and they are widely distributed, so the treatment methods are also different. Judging from the current domestic and international situation, the main ways to treat waste tires are direct use, production of recycled rubber and rubber powder, combustion use and pyrolysis use. How to achieve high-value utilization of waste tires is the key to solving black pollution and promoting resource recycling.
[0004] However, the catalysts currently used to prepare spiral nanocarbon fibers have disadvantages such as complex preparation process, high preparation cost, and easy agglomeration, which also limits the industrial application of spiral nanocarbon fibers. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a catalyst for preparing spiral nanocarbon fibers and its application, so as to solve the problems in the prior art of high batch production cost of spiral nanocarbon fibers, high catalyst production cost and easy agglomeration.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A catalyst for preparing spiral carbon nanofibers, wherein the catalyst is a soluble salt and is prepared by the following steps:
[0008] Step 1: dissolving LiCl, CoCl2 and citric acid in deionized water, heating to 55°C to 65°C and stirring for 4 to 7 hours until completely dissolved, and drying at 60-90°C to obtain powder; wherein the ratio of the sum of the amounts of LiCl and CoCl2 to the amount of citric acid is 1:(3 to 1), and the amounts of LiCl and CoCl2 are both greater than 0;
[0009] Step 2: Place the product obtained after drying in step 1 in a tube furnace, calcine at a high temperature of 550-650°C for 2-3 hours, and then ball-mill to obtain the catalyst Li x Co y Carbonate.
[0010] Preferably, in step 1, LiCl and CoCl2 are prepared in any molar ratio.
[0011] Preferably, the molar ratio of LiCl to CoCl2 is 1≤n LiCl / n CoCl2 ≤5.
[0012] The present invention also provides an application of a catalyst, wherein the catalyst is used to prepare spiral carbon nanofibers, specifically comprising the following steps:
[0013] S1: Refining tire rubber powder in an open mill for 3 to 5 minutes, then adding a catalyst and continuing to refine for 10 to 15 minutes, taking it out and crushing it to obtain treated rubber powder; wherein the mass ratio of the catalyst to the tire rubber powder is (1 to 2): (3 to 1);
[0014] S2: placing the rubber powder treated by S1 on a graphite substrate, then placing the graphite substrate in a tube furnace, introducing an inert gas to exhaust the air in the tube furnace, then heating to 500°C to 600°C, keeping the temperature for 2 to 3 hours, and then cooling to room temperature to obtain a crude product;
[0015] S3: The crude product obtained in S2 is ground into powder, added into ethanol solution for ultrasonic dissolution, filtered, washed and dried to obtain spiral nanocarbon fibers.
[0016] Preferably, the tire is a waste tire.
[0017] Preferably, the tire rubber powder has a mesh size of 30 to 200.
[0018] Preferably, the processed rubber powder has a mesh size of 100 to 200.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The catalyst of the present invention uses LiCl and CoCl2 as raw materials to prepare soluble Li x Co yCarbonate, this catalyst has good dispersibility and can improve the catalytic efficiency of growing spiral nanocarbon fibers; at the same time, the spiral nanocarbon fibers prepared by the prior art using metal and alloy catalysts require acid washing to remove residual catalysts, and this acid washing will destroy the performance and structure of the product, but the catalyst prepared by the present invention is a soluble salt, and the catalyst remaining in the spiral nanocarbon fibers can be removed by simple water washing. The subsequent treatment process is simple and feasible, and can effectively reduce the treatment cost, and is safe and environmentally friendly.
[0021] 2. The present invention uses tire rubber powder as a carbon source, which can improve the utilization value of waste tires. At the same time, the sulfur in the tire rubber powder can be used as an additive for growing spiral nanocarbon fibers; and x Co y Carbonate is used as a catalyst to increase the deposition rate of carbon atoms on the catalyst surface and improve the yield of spiral nanocarbon fibers. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the SEM image of the spiral nanocarbon fiber prepared in Example 6.
[0023] Figure 2 Li prepared in Example 1 x Co y XRD patterns of carbonates. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0025] 1. A catalyst for preparing helical carbon nanofibers
[0026] The catalyst of the present invention is a soluble salt, which is prepared by the following steps:
[0027] Step 1: dissolving LiCl, CoCl2 and citric acid in deionized water, heating to 55°C to 65°C and stirring for 4 to 7 hours until completely dissolved, and drying at 60-90°C to obtain powder; wherein the ratio of the sum of the amounts of LiCl and CoCl2 to the amount of citric acid is 1:(3 to 1), and the amounts of LiCl and CoCl2 are both greater than 0;
[0028] Step 2: Place the product obtained after drying in step 1 in a tube furnace, calcine at a high temperature of 550-650°C for 2-3 hours, and then ball-mill to obtain the catalyst Li x Co y Carbonate.
[0029] Since most of the catalysts used in the prior art are metal catalysts, this part of the catalysts not only has a complex preparation process, but also has a high production cost, and is prone to agglomeration and other phenomena. More importantly, the present invention finds that these catalysts will remain in the carbon nanotubes, so that the carbon nanotubes need to be subsequently treated. For example, in patent CN2019110966872, tires are used as carbon sources, catalysts and waste tire particles are evenly mixed, and carbon nanotubes are prepared by chemical vapor deposition at 700℃ to 900℃. The yield can reach more than 30%, realizing the high-value utilization of waste tires, which has great economic value and social benefits. However, the patent uses Ni-Co / Al2O3 bimetallic catalysts, which are more complicated to prepare and have higher production costs. Ni-Co metal residues are present in the prepared carbon nanotubes, which need to be removed by acid treatment. This also makes the subsequent treatment process more complicated. Not only is there a problem of waste acid after treatment, but the morphology of carbon nanotubes after acid treatment is also affected.
[0030] To this end, the present invention considers how to make the catalyst easier to remove from the spiral nanocarbon fibers, and unexpectedly found that the LiCl, CoCl2 and citric acid are selected as raw materials to prepare the Li x Co y Carbonate is a soluble salt, Li x Co y Carbonate can not only be used to prepare spiral nanocarbon fibers and improve the yield of the product, but also because this catalyst is a soluble salt, after the preparation is completed, only a simple water wash is needed to remove the catalyst remaining in the spiral nanocarbon fibers without destroying the performance and structure of the product. x Co y Carbonate can adjust the catalyst by adjusting the amount of LiCl and CoCl2 added, thereby obtaining a catalyst with different x and y values.
[0031] Embodiment 1:
[0032] Step 1: Dissolve LiCl, CoCl2 and citric acid in deionized water, heat to 60°C and stir for 6 hours until completely dissolved, and dry at 60-90°C to obtain powder; the amounts of LiCl, CoCl2 and citric acid are shown in Table 1.
[0033] Step 2: Place the product obtained after drying in step 1 in a tube furnace, calcine at a high temperature of 600°C for 2 to 3 hours, and then ball mill to obtain the catalyst Li x Co y Carbonate.
[0034] Figure 2 Li prepared in Example 1 x Co y XRD pattern of carbonate, in which Li x Co y The carbonate diffraction peak is sharp and has obvious characteristic peaks. Its diffraction peaks are basically consistent with the standard card PDF#76-2390 of Co2(CO)8 and the standard card PDF#72-1216 of Li2CO3, which indicates that Li x Co y Carbonate.
[0035] In other examples, materials were prepared according to Table 1, and the catalyst was prepared using the method of Example 1.
[0036] Table 1
[0037]
[0038]
[0039] 2. Application of a catalyst for preparing spiral nanocarbon fibers
[0040] Embodiment 6:
[0041] The catalyst prepared in Example 1 was used to prepare spiral carbon nanofibers, which specifically included the following steps:
[0042] S1: Refining tire rubber powder in an open mill for 3 to 5 minutes, then adding a catalyst and continuing to refine for 10 minutes, taking it out and crushing it to obtain treated rubber powder; wherein the mass ratio of the catalyst to the tire rubber powder is 1:2; the tire is a waste tire, the tire rubber powder is 30 to 200 meshes, and the treated rubber powder is 100 to 200 meshes.
[0043] S2: placing the rubber powder treated by S1 on a graphite substrate, then placing the graphite substrate in a tube furnace, introducing inert gas to exhaust the air in the tube furnace, then heating to 500° C., keeping the temperature for 2 to 3 hours, and then cooling to room temperature to obtain a crude product;
[0044] S3: Grind the crude product obtained in S2 into powder, add it into ethanol solution for ultrasonic dissolution, filter the dissolved solution, wash and dry the obtained solid to obtain spiral nanocarbon fiber.
[0045] The preparation methods of other embodiments 6 to 13 are consistent with that of embodiment 6, and the differences are shown in Table 2.
[0046] Table 2
[0047]
[0048] Through research, it is found that LiCl and CoCl2 can be configured in any molar ratio to obtain catalysts with different x and y values, which can be used to catalyze the preparation of spiral nanocarbon fibers. However, catalysts with different x and y values will have different effects on the yield and morphology of nanocarbon fibers. x Co y x and y in the carbonate also represent the amount of LiCl and CoCl2 added as raw materials. Under the premise that the reaction conditions remain unchanged, when the content of Li or Co in the catalyst is at a low level, although the catalyst can be used to prepare nano-carbon fibers, the yield is not high, and the morphology of the nano-carbon fibers is relatively complex, including straight fibers and spiral fibers; however, the content of Li in the catalyst gradually increases, and the yield also changes accordingly. The yield of nano-carbon fibers first gradually increases with the increase of Li content, but when the Li content reaches a certain value, the yield begins to decline.
[0049] As can be seen from Examples 6 to 8 in Table 2, the reaction temperature also affects the yield and morphology of the product. As the reaction temperature increases, the yield increases significantly, but when the reaction temperature reaches 600°C, the yield decreases, which indicates that a higher reaction temperature is not conducive to the formation of spiral nanocarbon fibers, and a higher temperature leads to the appearance of some straight fibers. The appearance of straight fibers causes the coexistence of spiral nanocarbon fibers and straight fibers in the spiral nanocarbon fiber material, which causes some properties of the spiral nanocarbon fibers to decrease, such as wave absorbing properties.
[0050] It can be seen from Examples 7, 9 to 12 in Table 2 that as the proportion of Li in the catalyst gradually increases, the yield fluctuates, but is still within a relatively high range overall. x Co y When x / y≥4, some straight fibers appear in the product.
[0051] In step S3 of Example 6, the crude product obtained in S2 was subjected to elemental analysis by EDS electron energy spectrum, and then the spiral nanocarbon fibers finally obtained after washing were subjected to elemental analysis. The contents of Co and Li in the products before and after washing are shown in Table 3:
[0052] Table 3
[0053]
[0054] It can be seen that the catalyst prepared by the present invention is a soluble salt, and the catalyst remaining in the spiral nano-carbon fiber can be removed by simple water washing. The subsequent treatment process is simple and feasible, and can effectively reduce the treatment cost, and is safe and environmentally friendly.
[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A catalyst for preparing spiral nanocarbon fibers, characterized in that: The catalyst is a soluble salt, which is prepared by the following steps: Step 1: dissolve LiCl, CoCl2 and citric acid in deionized water, heat to 55°C~65°C and stir for 4~7h until completely dissolved, and dry at 60-90°C to obtain powder; wherein the ratio of the sum of the amount of LiCl and CoCl2 to the amount of citric acid is 1:(3~1), and the amount of LiCl and CoCl2 is greater than 0; Step 2: Place the product obtained after drying in step 1 in a tube furnace, calcine at a high temperature of 550-650°C for 2-3 hours, and then ball-mill to obtain the catalyst Li x Co y Carbonates; The molar ratio of LiCl and CoCl2 is 1≤n LiCl / n CoCl2 ≤5.
2. An application of a catalyst, characterized in that: The catalyst as claimed in claim 1 is used to prepare helical nanocarbon fibers.
3. The use of the catalyst according to claim 2, characterized in that: The catalyst is used to prepare spiral carbon nanofibers, which specifically comprises the following steps: S1: Refining tire rubber powder in an open mill for 3-5 minutes, then adding a catalyst and continuing to refine for 10-15 minutes, taking it out and crushing it to obtain treated rubber powder; wherein the mass ratio of the catalyst to the tire rubber powder is (1-2):(3-1); S2: placing the rubber powder treated by S1 on a graphite substrate, then placing the graphite substrate in a tube furnace, introducing an inert gas to exhaust the air in the tube furnace, then heating to 500°C~600°C, keeping the temperature for 2~3h, and then cooling to room temperature to obtain a crude product; S3: The crude product obtained in S2 is ground into powder, added into ethanol solution for ultrasonic dissolution, filtered, washed and dried to obtain spiral nanocarbon fibers.
4. The use of the catalyst according to claim 3, characterized in that: The tire is a waste tire.
5. The use of the catalyst according to claim 3, characterized in that: The tire rubber powder has a mesh size of 30 to 200.
6. The use of the catalyst according to claim 3, characterized in that: The processed rubber powder is 100~200 mesh.