A method for dispersing graphene in a liquid system
Through repeated ball milling ultrasonic treatment and settlement layering technology, the problem of poor dispersion of graphene in liquid is solved, and efficient and uniform dispersion of graphene in lubricating oil is achieved, ensuring the performance of the dispersion liquid and the maintenance of liquid properties.
Patent Information
- Application Number
- CN202310166134.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-02-23
AI Technical Summary
Graphene is not easily dispersed uniformly in lubricating oil or water and is prone to agglomeration. Existing chemical dispersion methods may affect the properties of graphene or liquid systems.
Repeated ball milling ultrasonic treatment combined with settlement stratification technology is used to ensure uniform dispersion of graphene in the liquid system without the need to introduce other chemicals.
The efficient and uniform dispersion of graphene in the liquid system is achieved, the original properties of the liquid system are maintained, and the performance of graphene dispersion is improved.
Smart Images

Figure CN116199213B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of graphene, and in particular to a method for dispersing graphene in a liquid system. Background Art
[0002] Graphene is used in all walks of life due to its excellent properties. However, graphene is not easy to disperse evenly in liquids such as lubricating oil or water, and is easy to agglomerate, which affects its application in liquid systems. Particle size control and dispersion technology are the key to preparing graphene-containing dispersions. Nowadays, the dispersion problem of graphene is mainly solved by chemical dispersion methods, that is, using the dispersing effect of dispersants to make graphene dispersed evenly and stably in lubricating oil or water, but the disadvantage of this method is that the additional dispersant may affect the properties of graphene or the liquid system, thereby affecting the performance of the graphene dispersion. Summary of the invention
[0003] Based on this, the object of the present invention is to provide a method for dispersing graphene in a liquid system, which can improve the dispersibility of graphene in the liquid system without introducing other chemical substances.
[0004] The present invention relates to a method for dispersing graphene in a liquid system, comprising the following steps:
[0005] S1: putting graphene powder into liquid and mixing to obtain a first mixed liquid;
[0006] S2: subjecting the first mixed solution to ball milling ultrasonic treatment for more than three times to obtain a second mixed solution;
[0007] S3: allowing the second mixed liquid to settle and separate into layers, and taking at least a portion of the upper layer as the third mixed liquid;
[0008] S4: performing ball milling ultrasonic treatment on the third mixed solution for more than one time to obtain a graphene dispersion;
[0009] The ball milling ultrasonic treatment includes a ball milling treatment of adding grinding balls to the mixed solution for grinding and an ultrasonic treatment of subjecting the mixed solution to ultrasonic treatment.
[0010] The present invention efficiently breaks up the agglomerated graphene in the liquid system by repeated ball milling and ultrasonic treatment, and further ensures that the graphene is completely and evenly dispersed in the liquid system by sedimentation and stratification treatment and further ball milling and ultrasonic treatment. Based on this specific combination of physical methods, the dispersibility of graphene in the liquid system can be improved without introducing other chemical substances.
[0011] Furthermore, in the ball milling ultrasonic treatment in the above step S2, the grinding time of the ball milling treatment is more than 30 minutes.
[0012] Furthermore, in the ball milling ultrasonic treatment in the above step S2, the grinding time of the ball milling treatment is 30 to 120 minutes.
[0013] Furthermore, the grinding balls include 5% to 10% grinding balls with a diameter of 5 mm, 20% to 30% grinding balls with a diameter of 3 mm, 30% to 50% grinding balls with a diameter of 1 mm and 20% to 30% grinding balls with a diameter of 0.5 mm.
[0014] Furthermore, in the ball milling ultrasonic treatment in step S2, the ultrasonic treatment time is 30 to 120 minutes.
[0015] Furthermore, in the step S1, the graphene powder and the liquid are mixed by high-speed stirring at a stirring speed of 2000 r / min or more and a stirring time of 30 minutes or more.
[0016] Furthermore, in the ball milling ultrasonic treatment of step S4, the grinding time of the ball milling treatment is more than 60 minutes, and the ultrasonic treatment time is more than 60 minutes.
[0017] Furthermore, in the above step S3, the second mixed solution is allowed to settle and separate into layers by centrifugation or standing.
[0018] Furthermore, the above-mentioned liquid is lubricating oil.
[0019] On the other hand, the present invention also provides a graphene dispersion liquid, which is obtained by any of the above-mentioned dispersion methods.
[0020] For better understanding and implementation, the present invention is described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The graphene used in the examples and comparative examples of the present invention is shown in scanning electron microscope images.
[0022] Figure 2 The magnified images of graphene dispersions 1 to 9 obtained in Comparative Examples 1 to 9. Among them, (a-1) is a 50-fold magnified image of graphene dispersion 1; (a-2) is a 50-fold magnified image of graphene dispersion 2; (a-3) is a 50-fold magnified image of graphene dispersion 3; (b-1) is a 50-fold magnified image of graphene dispersion 4; (b-2) is a 50-fold magnified image of graphene dispersion 5; (b-3) is a 50-fold magnified image of graphene dispersion 6; (c-1) is a 200-fold magnified image of graphene dispersion 7; (c-2) is a 200-fold magnified image of graphene dispersion 8; (c-3) is a 200-fold magnified image of graphene dispersion 9.
[0023] Figure 3This is a 200-fold magnified image of the graphene dispersion 10 obtained in Example 1.
[0024] Figure 4 This is the infrared spectrum of the graphene dispersion 10 obtained in Example 1.
[0025] Figure 5 The graphene dispersion obtained in the comparative example and pure lubricating oil are subjected to a four-ball friction test and the steel ball wear spot image is shown.
[0026] Among them, (a) is the steel ball wear spot image of graphene dispersion 3; (b) is the steel ball wear spot image of graphene dispersion 6; (c) is the steel ball wear spot image of graphene dispersion 9; (d) is the steel ball wear spot image of pure lubricating oil.
[0027] Figure 6 This is a steel ball wear spot image after the graphene dispersion 10 obtained in Example 1 was subjected to a four-ball friction test. DETAILED DESCRIPTION
[0028] To solve the above problems, the present invention uses a purely physical method to improve the dispersibility of graphene in lubricating oil, and uses specific physical methods and combinations thereof to improve the agglomeration of graphene in a liquid system.
[0029] The present invention relates to a method for dispersing graphene in a liquid system, comprising the following steps:
[0030] S1: putting graphene powder into liquid and mixing to obtain a first mixed liquid;
[0031] S2: subjecting the first mixed solution to ball milling ultrasonic treatment for more than three times to obtain a second mixed solution;
[0032] S3: allowing the second mixed liquid to settle and separate into layers, and taking at least a portion of the upper layer liquid as the third mixed liquid;
[0033] S4: performing ball milling ultrasonic treatment on the third mixed solution for more than one time to obtain a graphene dispersion;
[0034] The ball milling ultrasonic treatment includes a ball milling treatment of adding grinding balls into the mixed solution for grinding and an ultrasonic treatment of performing ultrasonic treatment on the mixed solution.
[0035] Hereinafter, preferred implementations of the above steps will be described in detail.
[0036] For step S1: graphene powder is put into liquid and mixed to obtain a first mixed liquid.
[0037] Specifically, a proper amount of graphene powder can be weighed and placed in a container containing liquid, and the graphene can be uniformly mixed in the liquid manually or by machine to obtain a first mixed liquid. Preferably, the mixing is performed in the following manner: after the graphene powder and the liquid are preliminarily mixed by machine or manually at a low speed of less than 500 r / min, high-speed stirring is performed at a high speed of more than 2000 r / min for more than 30 minutes.
[0038] In this step, graphene powder refers to a single layer or a few layers of graphene, and the liquid can be a liquid system such as lubricating oil, water, and a mixture of oil and water. High-speed stirring treatment can be performed by mechanical stirring or magnetic stirring with a high-speed stirrer. In order to achieve a good dispersion effect, the stirring speed can be set to not less than 2000r / min. When the stirring speed is too high, if it is limited by the size of the container, it is easy to form a hollow vortex in the stirring container, thereby affecting the dispersion of graphene; the maximum stirring speed can be controlled according to the size of the container. In general, the stirring speed can be set to 2000-3000r / min. In the high-speed stirring treatment, if the stirring time is more than 30min, it is easy to obtain a uniformly mixed graphene mixture, which is conducive to subsequent dispersion treatment; when the stirring time exceeds 120min, the dispersion degree of the graphene powder is difficult to further improve. In order to take into account both the dispersion effect and the dispersion efficiency, the stirring time is preferably 30-120min.
[0039] For step S2: the first mixed solution is subjected to ball milling ultrasonic treatment for more than three times to obtain a second mixed solution.
[0040] Specifically, the ball milling ultrasonic treatment includes ball milling treatment and ultrasonic treatment, and the mixed solution can be first ball milled and then ultrasonically treated, or the mixed solution can be first ultrasonically treated and then ball milled. For example, the first mixed solution in step S1 can be poured into a clean and dry ball milling jar, and grinding balls with appropriate gradation can be added, and the grinding time is not less than 30 minutes; then, the ground mixed solution is subjected to ultrasonic (wave) treatment for not less than 30 minutes; the mixed solution obtained after ultrasonication is repeatedly subjected to the above ball milling and ultrasonic treatment for more than two times to obtain a second mixed solution.
[0041] In the ball milling ultrasonic treatment of this step, the grinding time of the ball milling treatment is not less than 30min, the ultrasonic treatment time is not less than 30min, and when the ball milling ultrasonic treatment is repeated for at least 3 times, the agglomerated graphene can be repeatedly ground and broken up in time, so as to efficiently and fully disperse the graphene in the liquid system. When each treatment time is too long, the improvement of the dispersion degree of graphene is extremely limited, and it is very likely to cause the performance changes of serious curling, folding deformation, etc. of graphene, so it is preferred that the grinding time of the ball milling treatment in each ball milling ultrasonic treatment is 30 to 120min, and the ultrasonic time of the ultrasonic treatment is 30 to 120min. In addition, when the ball milling ultrasonic treatment is repeated for more than 5 times, the dispersion effect is not greatly improved. For the consideration of both dispersion effect and dispersion efficiency, it is preferred to repeat the ball milling ultrasonic treatment for 3 to 5 times.
[0042] In the ball milling process, the grinding balls with appropriate gradation are preferably: 5% to 10% of the grinding balls with a diameter of 5 mm, 20% to 30% of the grinding balls with a diameter of 3 mm, 30% to 50% of the grinding balls with a diameter of 1 mm, and 20% to 30% of the grinding balls with a diameter of 0.5 mm. The grinding balls of such specifications are close to the particle size of the graphene powder, so that the grinding degree is finer, which can improve the dispersion efficiency of the graphene in the liquid. In addition, for example, the grinding balls with a diameter of 3 mm, a diameter of 1 mm, and a diameter of 0.5 mm can also be selected in a grinding ball gradation with a ratio of 1:2:3 or 2:3:5.
[0043] Ball milling is preferably carried out using a planetary high-energy ball mill. Grinding balls and grinding jars can be made of non-ferrous series grinding balls and grinding jars such as zirconium oxide and tungsten carbide to reduce the generation of impurities in the liquid system due to the wear of the grinding jar and grinding balls during the ball milling process. Especially for the liquid system of lubricating oil, iron-based grinding can easily cause iron filings to mix into the liquid system, reducing the lubricating performance of the lubricating oil. Non-ferrous grinding can avoid this problem. Ultrasonic treatment can be carried out using an ultrasonic disperser such as an immersion ultrasonic disperser. Optionally, the grinding speed is 600-1000r / min and the ultrasonic power is 600-1200W.
[0044] For step S3: allow the second mixed liquid to settle and separate into layers, and take at least a portion of the upper layer liquid as the third mixed liquid.
[0045] Specifically, the second mixed solution in step S2 is centrifuged or allowed to stand for 3 to 5 days to settle and separate into layers, and then at least a portion of the upper mixed solution is taken as the third mixed solution. Preferably, the upper layer of the upper liquid is taken as the third mixed solution, for example, three quarters of the upper layer, one half of the upper layer, etc. of the upper liquid is taken as the third mixed solution.
[0046] For step S4: the third mixed liquid is subjected to ball milling ultrasonic treatment for more than one time to obtain a graphene dispersion liquid.
[0047] Specifically, the third mixed solution in step S3 can be subjected to ball milling for no less than 60 minutes, and then ultrasonically treated for more than 60 minutes, and the ball milling and ultrasonic treatment is performed more than once. Similarly, based on the dispersion efficiency, effect and the reason of avoiding the change of graphene properties, the ball milling time and ultrasonic dispersion time are preferably 60 to 120 minutes, and the number of ball milling and ultrasonic treatment is preferably 1 to 3 times.
[0048] In each treatment of the above steps, the temperature in each treatment can be controlled between the freezing point and the boiling point of the liquid system. When the treatment temperature is 15°C to 100°C, the dispersion efficiency can be further improved while ensuring that the liquid system maintains its original properties. Each treatment can be controlled in an intermittent treatment manner to be within the desired range. In this case, the treatment time of each treatment is the effective treatment time for actually performing the treatment.
[0049] The method for dispersing graphene in a liquid system involved in the present invention can efficiently break up the agglomerated graphene in the liquid system by repeated ball milling and ultrasonic treatment, and further, by sedimentation and stratification treatment and subsequent ball milling and ultrasonic treatment, it is possible to ensure that a graphene dispersion liquid in which the graphene is completely and evenly dispersed in the liquid system is obtained. The graphene dispersion method provided by the present invention does not require the addition of other chemical reagents, and can fully and evenly disperse the graphene in the liquid system while ensuring that the properties of the graphene dispersion liquid are not changed.
[0050] The following examples and comparative examples are used to further illustrate the implementation of the method of the present invention and its effects. The following examples are only examples of the present invention and do not limit the scope of the present invention.
[0051] Comparative Examples 1 to 3 (High-speed stirring)
[0052] Comparative Examples 1 to 3 only use high-speed stirring to disperse graphene, specifically: 100 mL of lubricating oil (Shell HX75W-40 lubricating oil, produced by Shell Hong Kong Limited, the same below) is measured and placed in a container, and a high-speed disperser (GFJ-0.4 type, produced by Shanghai Modern Environmental Engineering Technology Co., Ltd., the same below) is used to stir and mix the lubricating oil in the container at a speed of 150 r / min, and 10 mg of graphene (produced by Nanjing Jicang Nano Technology Co., Ltd., as shown in the electron microscope image) is added to the lubricating oil. Figure 1 As shown, the same below). After all the graphene is added, the speed is slowly increased to 2000r / min, and high-speed stirring is performed at room temperature (about 18°C) for a certain period of time to obtain a graphene dispersion. Among them, the high-speed stirring time in Comparative Example 1 is 30min; the high-speed stirring time in Comparative Example 2 is 60min; and the high-speed stirring time in Comparative Example 3 is 120min. Through Comparative Examples 1 to 3, graphene dispersions 1 to 3 are obtained respectively.
[0053] Comparative Examples 4 to 6 (ultrasonic treatment)
[0054] Comparative Examples 4 to 6 only use ultrasonic treatment to disperse graphene, specifically: first, measure 100mL of lubricating oil into a container, then weigh 10mg of graphene and add it to the lubricating oil at a speed of 150r / min for mixing. Set the ultrasonic dispersion equipment (SCIENTZ-1500F ultrasonic disperser, produced by Ningbo Xinzhi Biotechnology Co., Ltd., the same below) to start 15s and stop 20s in an intermittent working mode to control the processing temperature below 80°C, and effectively disperse for a certain period of time under the condition of a power of 600W to obtain a graphene dispersion. Among them, the ultrasonic time in Comparative Example 4 is 30min; the ultrasonic time in Comparative Example 5 is 60min; and the ultrasonic time in Comparative Example 6 is 120min. Through Comparative Examples 4 to 6, graphene dispersions 4 to 6 are obtained respectively.
[0055] Comparative Examples 7 to 9 (Ball Milling)
[0056] Comparative Examples 7 to 9 only use ball milling to disperse graphene, specifically: first, measure 100mL of lubricating oil and put it in a container, then weigh 10mg of graphene and add it to the lubricating oil at a speed of 150r / min for mixing. Add graded grinding balls (zirconia grinding balls with a diameter of 5mm account for 5%, 3mm account for 20%, 1mm account for 45%, and 0.5mm account for 30%, the same below) to the grinding jar, then pour the mixed solution of graphene and lubricating oil into the grinding jar, cover the grinding jar, put it into a high-energy ball mill (Pulverisette 7 type micro high-energy ball mill, produced by Fritsch Company, Germany, the same below), set the speed to 600r / min, work for 5min and stop for 3min, effectively disperse for a certain time, and obtain a graphene dispersion. Among them, the grinding time in Comparative Example 7 is 30min; the grinding time in Comparative Example 8 is 60min; the grinding time in Comparative Example 9 is 120min. Through Comparative Examples 7 to 9, graphene dispersions 7 to 9 were obtained, respectively.
[0057] Example 1
[0058] Example 1: Graphene is dispersed using the method of the present invention, specifically: first, 100 mL of lubricating oil is measured and put into a container, and the lubricating oil in the container is stirred at a speed of 150 r / min using a high-speed disperser. At the same time, 10 mg of graphene is added to the lubricating oil. After all the graphene is added, the speed is slowly increased to 2000 r / min, and stirred at high speed for 30 minutes at room temperature (about 18°C) to obtain a first mixed solution. Add graded grinding balls to the grinding jar, then pour the first mixed liquid into the grinding jar, cover the grinding jar, put it into a high-energy ball mill, set the speed to 600 r / min, work for 5 min and stop for 3 min, and effectively disperse for 30 min; then, set the ultrasonic dispersion equipment to an intermittent working mode of starting for 15 s and stopping for 20 s to control the temperature below 80°C, effectively disperse for 30 min at a power of 600 W, repeat the above ball milling ultrasonic treatment for a total of 3 times to obtain a second mixed liquid; then, use a centrifuge to centrifuge the second mixed liquid at 3000 r / min for 20 min, take three quarters of the upper liquid as the third mixed liquid; put the third mixed liquid into a high-energy ball mill and grind it for 60 min, then ultrasonicate it for 60 min to obtain a graphene dispersion 10.
[0059] Since there is currently no parameter or standard suitable for measuring the dispersion degree of graphene, the present invention evaluates the dispersion method of each embodiment and comparative example by directly observing the dispersion degree of the graphene dispersion and measuring the properties of the graphene dispersion.
[0060] [Observation of dispersion]
[0061] Using a metallographic fluorescence microscope (DM6 M, manufactured by Leica, Germany, the same below), the graphene dispersions 1 to 6 obtained in Comparative Examples 1 to 6 were observed at a magnification of 50 times, and the graphene dispersions 7 to 10 obtained in Comparative Examples 7 to 9 and Example 1 were observed at a magnification of 200 times. The magnified images of the graphene dispersions 1 to 9 are shown in Figure 2 ,in, Figure 2 (a-1) to (a-3) correspond to graphene dispersions 1 to 3, respectively. Figure 2 (b-1) to (b-3) correspond to graphene dispersions 4 to 6, respectively. Figure 2 (c-1) to (c-3) correspond to graphene dispersions 7 to 9, respectively. An enlarged image of graphene dispersion 10 is shown in Figure 3 .
[0062] [Component Analysis]
[0063] Pure lubricating oil and graphene dispersion 10 were placed in a Fourier transform infrared spectrometer (IS50 Fourier transform infrared spectrometer, produced by Thermo Fisher Scientific, USA) to analyze their components. The results are shown in Figure 4 .
[0064] [Performance test]
[0065] Using a four-ball friction tester (MRS-10H, produced by Jinan Chenda Testing Machine Manufacturing Co., Ltd.), under the conditions of oil box temperature of 75℃±2, servo motor speed of 1200±60r / min, test time of 3600±60s, and pressure of 392±2N, the friction coefficients of pure lubricating oil without adding graphene and graphene dispersions 3, 6, 9, and 10 were measured 5 times each, and the average value and standard deviation were calculated. Table 1 shows the friction coefficient values, average values, and standard deviations obtained by the measurement.
[0066] The wear spot diameters of the steel balls that have completed the complete test in Table 1 were measured, and the wear spot diameter values (unit: mm) as well as their average values and standard deviations are shown in Table 2. In addition, the wear spot morphology of each steel ball was observed using a metallographic fluorescence microscope, and the results are shown in Figure 5 and Figure 6 .in, Figure 5 (a) to (d) are the steel ball wear spot images after the four-ball friction test of graphene dispersion 3, graphene dispersion 6, graphene dispersion 9, and pure lubricating oil, respectively. Figure 6 This is the steel ball wear spot image after the four-ball friction test of graphene dispersion 10.
[0067]
Table 1
[0068] Number of tests 1 2 3 4 5 average value Standard Deviation Graphene dispersion 3 0.106 0.104 — — 0.108 0.106 — Graphene dispersion 6 0.104 0.103 0.107 0.105 — 0.105 — Graphene dispersion 9 0.106 0.102 0.107 0.106 0.103 0.105 0.0022 Graphene dispersion 10 0.105 0.103 0.103 0.104 0.105 0.104 0.0010 Pure lubricating oil 0.106 0.105 0.106 0.104 0.105 0.105 0.0008
[0069] *“—” indicates that the test was not completed due to a sudden increase in friction causing the equipment to shut down for protection.
[0070]
Table 2
[0071] Number of tests 1 2 3 4 5 average value Standard Deviation Graphene dispersion 3 0.630 0.643 — — 0.672 0.648 0.0215 Graphene dispersion 6 0.618 0.641 0.651 0.631 — 0.635 0.0141 Graphene dispersion 9 0.607 0.646 0.631 0.629 0.618 0.626 0.0147 Graphene dispersion 10 0.626 0.621 0.635 0.614 0.604 0.620 0.0118 Pure lubricating oil 0.643 0.616 0.633 0.638 0.620 0.630 0.0116
[0072] The results of observing each graphene dispersion using a metallographic fluorescence microscope are as follows: Figure 2 As shown, the horizontal comparison shows that under the same processing time, Figure 2 The dispersion of graphene in (c-1) to (c-3) is higher than Figure 2 (b-1)~(b-3), higher than Figure 2 (a-1) to (a-3), which means that ultrasonic treatment has a better dispersion effect on graphene than high-speed stirring treatment, and ball milling is better than ultrasonic treatment. Vertical comparison shows that the increase in time in each treatment is conducive to the dispersion of graphene, but the dispersion effect on graphene is limited as time increases. On the other hand, by comparing Figure 2 (c-1)~(c-3) and Figure 3It can be seen that the dispersion degree of the graphene dispersion 10 obtained in Example 1 is further better than that of the graphene dispersions 6 to 9 that have only been subjected to ball milling treatment.
[0073] As shown in Table 1, the test results of the four-ball friction test were not completed twice for the graphene dispersion 3 and once for the graphene dispersion 6. This is because there are undispersed agglomerated graphene in the graphene dispersion. The agglomerated graphene particles suddenly enter between the friction surfaces of the steel balls, breaking the original balance and causing a sudden increase in friction, which causes the equipment to shut down. This also shows that high-speed stirring or ultrasonic treatment alone cannot disperse agglomerated graphene well.
[0074] In Table 1, by comparing the standard deviations of the friction coefficients of the various dispersions, it can be seen that the fluctuation of the friction coefficient of the graphene dispersion 10 is smaller than that of the graphene dispersion 9 and is extremely close to that of pure lubricating oil, indicating that the dispersion of graphene in the graphene dispersion 10 is extremely uniform. On the other hand, by comparing the average values of the friction coefficients, it can be seen that the friction coefficients of the graphene dispersions 3, 6, and 9 are all higher than that of pure lubricating oil; the friction coefficient of the graphene dispersion 10 obtained in Example 1 is not only lower than the friction coefficients of the graphene dispersions 3, 6, and 10, but also lower than that of pure lubricating oil; it can be seen that the graphene dispersion obtained by dispersing graphene in lubricating oil by the method of Example 1 involved in the present invention can improve the lubricating effect of the lubricating oil.
[0075] In the wear spot measurement results shown in Table 2, it can be seen from the standard deviation that the wear spot diameters of graphene dispersions 3, 6, and 9 fluctuate greatly, which is related to the presence of a small amount of agglomerated graphene that has not been dispersed in the dispersion; while the data fluctuation of graphene dispersion 10 is almost consistent with the data fluctuation of pure lubricating oil, indicating that there is almost no agglomerated graphene in graphene dispersion 10, and graphene is fully and evenly dispersed in the lubricating oil. On the other hand, the comparison of the average values of the wear spot diameters shows that the wear spot diameters of graphene dispersions 9 and 10 are both smaller than the wear spot diameter of pure lubricating oil, which shows that graphene dispersions 9 and 10 can both improve the wear resistance of lubricating oil; and the wear spot diameter of graphene dispersion 10 is smaller, indicating that its wear resistance is better.
[0076] also, Figure 5 , Figure 6 The wear spots of various graphene dispersions and pure lubricating oil are shown. Figure 5 The wear spots of the steel ball corresponding to the lubricating oil shown in (d) are relatively flat, without obvious scratches, and their shapes are mostly round; Figure 5 The steel ball wear spots corresponding to the graphene dispersion 3 shown in (a) are uneven and have obvious deeper wear marks, which may be caused by the particles formed by the undispersed graphene. Figure 5 (b) The steel ball corresponding to the graphene dispersion 6 shown, Figure 5The probability of the steel ball corresponding to the graphene dispersion 9 shown in (c) having a deeper wear mark gradually decreases. Figure 6 The wear spots corresponding to the graphene dispersion 10 shown in FIG. 1 are less likely to show obvious wear marks than those of the graphene dispersions 6 and 9. Figure 5 The wear spots and scars corresponding to the lubricating oil shown in (d) are of similar degree, indicating that the graphene in the graphene dispersion 10 is extremely uniformly dispersed.
[0077] For the results of infrared spectroscopy analysis, such as Figure 4 As shown, the infrared spectra of the graphene dispersion 10 and the pure lubricating oil are basically consistent, indicating that the dispersion method of Example 1 will not cause the composition of the lubricating oil to change.
[0078] According to the above test results, direct observation, standard deviation in each test, and wear spot morphology all show that there is almost no agglomerated graphene in the graphene dispersion 10, and the dispersion of graphene is extremely uniform; in addition, the infrared results show that the components of graphene and lubricating oil in the graphene dispersion 10 have not changed. It can be seen that the graphene dispersion method involved in the present invention can efficiently and fully break up the agglomerated graphene in the liquid, making it uniformly dispersed in the liquid, and will not change the properties of the liquid itself.
[0079] Furthermore, the results of the friction coefficient and the wear spot diameter show that the graphene dispersion 10 obtained in Example 1 also has excellent lubrication effect and anti-wear performance. This shows that when graphene is dispersed in lubricating oil by the dispersion method of the present invention, a graphene dispersion with excellent lubrication effect and anti-wear performance can be obtained.
[0080] The dispersion method of the present invention is particularly suitable for dispersing graphene in a liquid system with a graphene concentration of less than 0.5 mg / mL, and graphene can be fully, uniformly and efficiently dispersed in the liquid system without introducing other chemical substances.
[0081] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for dispersing graphene in a liquid system, characterized in that: The following steps are involved: S1: putting graphene powder into a liquid, and mixing the graphene powder and the liquid by high-speed stirring at a stirring speed of 2000 r / min or more and a stirring time of 30 minutes or more to obtain a first mixed liquid, wherein the liquid is any one of oil, water or an oil-water mixture; S2: subjecting the first mixed solution to ball milling ultrasonic treatment for more than three times to obtain a second mixed solution, wherein the ball milling time is more than 30 minutes, and the ultrasonic treatment time is 30 to 120 minutes; S3: allowing the second mixed liquid to settle and separate into layers, and taking at least a portion of the upper layer liquid as the third mixed liquid; S4: subjecting the third mixed solution to ball milling and ultrasonic treatment for more than one time to obtain a graphene dispersion, wherein the ball milling time is more than 60 minutes, and the ultrasonic treatment time is more than 60 minutes; The ball milling ultrasonic treatment includes a ball milling treatment of adding grinding balls into the mixed solution for grinding and an ultrasonic treatment of performing ultrasonic treatment on the mixed solution.
2. The method for dispersing graphene in a liquid system according to claim 1, characterized in that: In the ball milling ultrasonic treatment of step S2, the grinding time of the ball milling treatment is 30 to 120 minutes.
3. The method for dispersing graphene in a liquid system according to claim 2, characterized in that: The grinding balls include 5% to 10% grinding balls with a diameter of 5 mm, 20% to 30% grinding balls with a diameter of 3 mm, 30% to 50% grinding balls with a diameter of 1 mm and 20% to 30% grinding balls with a diameter of 0.5 mm.
4. The method for dispersing graphene in a liquid system according to claim 1, characterized in that: In the step S3, the second mixed solution is allowed to settle and separate into layers by centrifugation or standing.
5. The method for dispersing graphene in a liquid system according to claim 1, characterized in that: The liquid is lubricating oil.
6. A graphene dispersion, characterized in that: Obtained by any one of the dispersion methods described in claims 1 to 5.