A method for preparing an environmentally friendly high-strength and high-wear-resistant cable

By using nano-attapulgite, modified cerium dioxide powder and other materials in cable materials to replace traditional lead and cadmium components, the problem of insufficient mechanical properties and low-temperature resistance of cable materials is solved, and environmentally friendly, high-strength and high-wear resistance are achieved. Preparation of cable materials suitable for the demanding applications of modern cables.

CN116199983BActive Publication Date: 2024-10-01JIANGXI HUCHANG CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310141517.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-21
Publication Date
2024-10-01
Estimated Expiration
2043-02-21

AI Technical Summary

Technical Problem

Existing polyvinyl chloride cable materials contain lead and cadmium components, which cause harm to the environment, and their mechanical properties and low-temperature resistance are insufficient, making it difficult to meet the high strength and durability requirements of modern cables.

Method used

Using materials such as nano attapulgite, modified ceria powder, alumina powder, light calcium carbonate powder, zinc borate, etc., combined with specific formula ratios and process flows, an environmentally friendly, high-strength and high-wear-resistant cable material is prepared , replacing traditional lead and cadmium components, and improving the dispersion and mechanical properties of the material through the preparation method of modified cerium dioxide powder.

Benefits of technology

The prepared cable material has good mechanical properties and low-temperature resistance, replaces traditional lead and cadmium components, reduces environmental harm, and is suitable for manufacturing wires and cables requiring high strength and durability, especially for applications in low-temperature environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing an environmentally friendly high-strength and high-wear-resistant cable, comprising: (1) weighing each component of a cable material, wherein the component comprises polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; (2) polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder are uniformly mixed to obtain a mixture A; (3) mixture A is added to the remaining materials to obtain a mixture B; (4) banburying, granulation, obtaining a finished cable material, and the finished cable material is made into a sheath to obtain a cable. The cable material formula prepared by the method of the present invention replaces the lead and cadmium components in the traditional formula of polyvinyl chloride cable material, and reduces the harm of wires and cables to the surrounding environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wire and cable materials, and in particular to a method for preparing an environmentally friendly high-strength and high-wear-resistant cable. Background Art

[0002] Wires and cables are called the "arteries" and "nerves" of the national economy, and their products are widely used in the fields of construction, transportation, power plants, automobiles, petrochemicals, etc. Polyvinyl chloride (PVC) is one of the most widely used plastics in the world. It is inexpensive and has excellent corrosion resistance and electrical insulation, especially flame resistance and self-extinguishing properties. Therefore, polyvinyl chloride has been widely used in the production of cable materials. It has long occupied an important position in the insulation and protective materials of wires and cables, and is widely used in various types of wire and cable insulation and sheath materials. Summary of the invention

[0003] To this end, the present invention provides a method for preparing an environmentally friendly high-strength and high-wear-resistant cable, comprising the following steps:

[0004] (1) Weighing components of cable materials, including polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid;

[0005] (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A;

[0006] (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, stirring evenly after the addition is completed to obtain a mixture B;

[0007] (4) The mixture B is kneaded at a temperature of 100 to 110° C. for 7 to 10 minutes, and then mixed and granulated in an extruder at an extrusion temperature of 150 to 180° C. to obtain a finished cable material. During the cable manufacturing process, the finished cable material is made into a sheath to obtain the environmentally friendly high-strength and high-wear-resistant cable.

[0008] Furthermore, the preparation method of the modified cerium dioxide powder is:

[0009] Step 1, preparing an aqueous solution of cerium nitrate and ethylene glycol, placing the aqueous solution of cerium nitrate and ethylene glycol in a reactor and keeping the temperature at 65±5°C in a water bath, then stirring the aqueous solution of cerium nitrate and ethylene glycol, and dropping ammonia water into the solution during the stirring process until no precipitation is generated, then sealing the reactor, heating to 120±5°C and keeping the temperature for 4-5h, air cooling to room temperature after the insulation is completed, opening the reactor, separating the solid and liquid, washing the solid phase with ethanol, and drying to obtain a solid phase A;

[0010] Step 2: prepare a composite ethanol solution of zinc chloride, antimony chloride and tin chloride, immerse the solid phase A in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride, let it stand for 5 to 6 minutes, then separate the solid and liquid, dry the solid phase at 100 to 120° C. for more than 10 minutes, and then calcine at 500 to 550° C. for more than 15 minutes; then air-cool to room temperature, immerse it in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride again and let it stand for 5 to 6 minutes, then separate the solid and liquid, dry the solid phase at 100 to 120° C. for more than 10 minutes, and then calcine at 500 to 550° C. for more than 15 minutes; repeat the above immersion, solid-liquid separation, drying and calcination process for a total of 10 to 12 groups, calcine for the last time for 1 to 2 hours, and then air-cool to room temperature to obtain solid phase B;

[0011] Step 3: prepare an aqueous solution of anhydrous ethanol, add the solid phase B to the aqueous solution of anhydrous ethanol and stir to form a suspension, add isopropyl tri(dioctyl pyrophosphate acyloxy) titanate to the suspension, and after the addition is completed, keep the suspension in a water bath at a constant temperature of 55±5°C, keep it warm and stir for more than 1h, then filter it, and dry it at 60°C to obtain a solid phase C;

[0012] Step 4: Disperse the solid phase C in ethanol to form an alcohol suspension, add coupling agent KH-550 to the alcohol suspension under stirring, continue stirring for more than 10 hours after the addition is completed, separate the solid and liquid, wash the solid phase with deionized water, dry it, and obtain a solid phase D, disperse the solid phase D in an ethanol solution to obtain an alcohol mixture, place the alcohol mixture in a nitrogen atmosphere, keep the water bath temperature at 80±5°C, then add potassium ethyl xanthate to the alcohol mixture, and continue to stir under nitrogen after the addition is completed. The mixture is stirred at a constant temperature of 80±5°C in an atmosphere for more than 12 hours, then air-cooled to room temperature, the solid-liquid is separated, the solid phase is washed with ethanol, and dried; the dried solid phase is dispersed in N,N-dimethylformamide, and then the temperature is kept constant at 60±5°C in a water bath in a nitrogen atmosphere, and methyl methacrylate and azobisisobutyronitrile are added in sequence. After the addition is completed, the mixture is kept warm at 60±5°C in a nitrogen atmosphere for more than 12 hours, then air-cooled to room temperature, the solid-liquid is separated, the solid phase is washed with ethanol, and dried to obtain the modified cerium dioxide powder.

[0013] Furthermore, the components are calculated by weight as follows: 100 parts of polyvinyl chloride resin, 10 to 20 parts of nano-attapulgite, 15 to 20 parts of dioctyl cyclohexane-1,2-dicarboxylate, 10 to 15 parts of trioctyl phosphite, 25 to 35 parts of nitrile rubber powder, 10 to 16 parts of alumina powder, 10 to 13 parts of light calcium carbonate powder, 12 to 20 parts of modified cerium dioxide powder, 5 to 10 parts of zinc borate, 0.5 to 0.8 parts of dilauryl thiodipropionate, 1 to 2 parts of 2,6-di-tert-butyl-4-methylphenol, 5 to 9 parts of vinyl trimethoxysilane, 3 to 6 parts of antioxidant TPPD, 10 to 14 parts of wollastonite powder, and 2 to 5 parts of stearic acid.

[0014] Furthermore, in the aqueous solution of cerium nitrate and ethylene glycol, the concentration of cerium nitrate is 3-5 g / 100 mL, the volume fraction of ethylene glycol is 50%, and the mass percentage of the solute in the ammonia water is 25%.

[0015] Furthermore, in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride, the concentration of zinc chloride is 10-16 g / L, the concentration of antimony chloride is 8-12 g / L, the concentration of tin chloride is 3-5 g / L, and the solvent is ethanol.

[0016] Furthermore, in the step three, the volume fraction of anhydrous ethanol in the aqueous solution of anhydrous ethanol is 50%; the solid-liquid mass ratio of the solid phase B added to the aqueous solution of anhydrous ethanol is solid phase B / anhydrous ethanol aqueous solution = 1 / 10, and the added mass of the isopropyl tri(dioctyl pyrophosphate) titanate is 5% to 8% of the mass of the solid phase B.

[0017] Furthermore, in the step 4, the solid-liquid mass ratio of the solid phase C dispersed in ethanol is solid phase C / ethanol=1:20; the added mass of the coupling agent KH-550 is 30% to 40% of the mass of the solid phase C; the solid-liquid mass ratio of the solid phase D dispersed in the ethanol solution is solid phase D / ethanol=1:20; the added mass of the potassium ethyl xanthate is 1.6 to 2.0 times the mass of the solid phase D; the solid-liquid mass ratio of the dried solid phase dispersed in N,N-dimethylformamide is solid / liquid=1:20; the mass ratio of the added mass of methyl methacrylate and azobisisobutyronitrile to the solid phase D is methyl methacrylate:azobisisobutyronitrile:solid phase D=3 to 4:0.01 to 0.02:1.

[0018] The beneficial effects of the present invention are that the cable material prepared by the method of the present invention has good mechanical properties and low temperature resistance and a wide range of applications, and replaces the lead and cadmium components in the traditional formula of polyvinyl chloride cable materials, reducing the harm of wires and cables to the surrounding environment. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with the embodiments.

[0020] Example 1

[0021] A method for preparing an environmentally friendly high-strength and high-wear-resistant cable material for manufacturing a cable sheath comprises the following steps:

[0022] (1) Weighing the components of the cable material, the components include polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; each component is calculated by weight The invention comprises: 100 parts of polyvinyl chloride resin, 10 parts of nano-attapulgite, 15 parts of dioctyl cyclohexane-1,2-dicarboxylate, 10 parts of trioctyl phosphite, 25 parts of nitrile rubber powder, 10 parts of alumina powder, 10 parts of light calcium carbonate powder, 12 parts of modified cerium dioxide powder, 5 parts of zinc borate, 0.5 parts of dilauryl thiodipropionate, 1 part of 2,6-di-tert-butyl-4-methylphenol, 5 parts of vinyl trimethoxysilane, 3 parts of antioxidant TPPD, 10 parts of wollastonite powder and 2 parts of stearic acid.

[0023] (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A;

[0024] (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, stirring evenly after the addition is completed to obtain a mixture B;

[0025] (4) The mixture B is kneaded at a temperature of 105±5°C for 8 minutes, and then mixed and granulated in an extruder at an extrusion temperature of 170°C to obtain a finished cable material. During the cable manufacturing process, the finished cable material is made into a sheath to obtain the environmentally friendly high-strength and high-wear-resistant cable.

[0026] Wherein, the preparation method of the modified cerium dioxide powder is:

[0027] Step 1, preparing an aqueous solution of cerium nitrate and ethylene glycol, wherein the concentration of cerium nitrate is 3g / 100mL and the volume fraction of ethylene glycol is 50%; placing the aqueous solution of cerium nitrate and ethylene glycol in a reactor and keeping the temperature at 65±5°C in a water bath, then stirring the aqueous solution of cerium nitrate and ethylene glycol at 50r / min, and adding ammonia water dropwise to the solution during the stirring process until no precipitation is generated, wherein the mass percentage of the solute in the ammonia water is 25%; then closing the reactor, heating to 120±5°C and keeping the temperature for 4h, air cooling to room temperature after the end of the keeping temperature, opening the reactor, separating the solid and liquid, washing the solid phase with ethanol, and drying to obtain a solid phase A;

[0028] Step 2, preparing a composite ethanol solution of zinc chloride, antimony chloride and tin chloride, wherein the concentration of zinc chloride is 10g / L, the concentration of antimony chloride is 8g / L, the concentration of tin chloride is 3g / L, and the solvent is ethanol; soaking the solid phase A in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride, standing for 5min, then separating the solid and liquid, drying the solid phase at 100°C for 10min, and then calcining at 520°C for 15min; then air cooling to room temperature, soaking in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride again and standing for 5min, then separating the solid and liquid, drying the solid phase at 100°C for 10min, and then calcining at 520°C for 15min; repeating the above soaking, solid-liquid separation, drying and calcining process for a total of 10 groups, calcining for the last time for 1h, and then air cooling to room temperature to obtain solid phase B;

[0029] Step 3, preparing an aqueous solution of anhydrous ethanol, wherein the volume fraction of anhydrous ethanol in the aqueous solution of anhydrous ethanol is 50%; adding the solid phase B to the aqueous solution of anhydrous ethanol and stirring to form a suspension, wherein the solid-liquid mass ratio of the solid phase B added to the aqueous solution of anhydrous ethanol is solid phase B / the aqueous solution of anhydrous ethanol=1 / 10; adding isopropyl tri(dioctyl pyrophosphate acyloxy) titanate to the suspension, wherein the added mass of isopropyl tri(dioctyl pyrophosphate acyloxy) titanate is 5% of the mass of the solid phase B; after the addition is completed, the suspension is heated to 55±5°C in a water bath, stirred at 60r / min for 1h, then filtered, and dried at 60°C to obtain a solid phase C;

[0030] Step 4: Disperse the solid phase C in ethanol to form an alcohol suspension, the solid-liquid mass ratio of the solid phase C dispersed in ethanol is solid phase C / ethanol=1:20; add coupling agent KH-550 to the alcohol suspension under 60r / min stirring, and the added mass of coupling agent KH-550 is 30% of the mass of the solid phase C; after the addition is completed, continue stirring at 60r / min for 10h, separate the solid and liquid, wash the solid phase with deionized water, dry it, obtain solid phase D, disperse the solid phase D in ethanol solution to obtain an alcohol mixture, the solid-liquid mass ratio of the solid phase D dispersed in the ethanol solution is solid phase D / ethanol=1:20; place the alcohol mixture in a nitrogen atmosphere, keep the water bath temperature at 80±5°C, and then add potassium ethyl xanthate to the alcohol mixture, the added mass of potassium ethyl xanthate is 1% of the mass of the solid phase D. .6 times; after the addition is completed, continue to stir at a constant temperature of 80±5℃ and 60r / min for 12h in a nitrogen atmosphere, then air-cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry; the dried solid phase is dispersed in N,N-dimethylformamide, and the solid-liquid mass ratio of the solid phase dispersed in N,N-dimethylformamide is solid / liquid=1:20; then keep the temperature in a water bath at 60±5℃ in a nitrogen atmosphere, and then add methyl methacrylate and azobisisobutyronitrile in sequence, the mass ratio of the added mass of methyl methacrylate and azobisisobutyronitrile to the solid phase D is methyl methacrylate: azobisisobutyronitrile: solid phase D=3:0.01:1; after the addition is completed, keep warm at 60±5℃ in a nitrogen atmosphere for 12h, then air-cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry to obtain the modified cerium dioxide powder.

[0031] Example 2

[0032] A method for preparing an environmentally friendly high-strength and high-wear-resistant cable material for manufacturing a cable sheath comprises the following steps:

[0033] (1) Weighing the components of the cable material, the components include polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; the weight percentage of each component is as follows: polyvinyl chloride resin 100 parts, nano-attapulgite 14 parts, dioctyl cyclohexane-1,2-dicarboxylate 17 parts, trioctyl phosphite 12 parts, nitrile rubber powder 28 parts, alumina powder 13 parts, light calcium carbonate powder 11 parts, modified cerium dioxide powder 15 parts, zinc borate 7 parts, dilauryl thiodipropionate 0.6 parts, 2,6-di-tert-butyl-4-methylphenol 1 part, vinyl trimethoxysilane 7 parts, antioxidant TPPD 4 parts, wollastonite powder 12 parts, stearic acid 3 parts;

[0034] (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A;

[0035] (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, stirring evenly after the addition is completed to obtain a mixture B;

[0036] (4) The mixture B is kneaded at a temperature of 105±5°C for 8 minutes, and then mixed and granulated in an extruder at an extrusion temperature of 170°C to obtain a finished cable material. During the cable manufacturing process, the finished cable material is made into a sheath to obtain the environmentally friendly high-strength and high-wear-resistant cable.

[0037] Wherein, the preparation method of the modified cerium dioxide powder is:

[0038] Step 1, preparing an aqueous solution of cerium nitrate and ethylene glycol, wherein the concentration of cerium nitrate is 4g / 100mL and the volume fraction of ethylene glycol is 50%; placing the aqueous solution of cerium nitrate and ethylene glycol in a reactor and keeping the temperature at 65±5°C in a water bath, then stirring the aqueous solution of cerium nitrate and ethylene glycol at 50r / min, and dropping ammonia water into the solution during the stirring process until no precipitation is generated, wherein the mass percentage of the solute in the ammonia water is 25%; then closing the reactor, heating to 120±5°C and keeping the temperature for 4h, air cooling to room temperature after the insulation is completed, opening the reactor, separating the solid and liquid, washing the solid phase with ethanol, and drying to obtain a solid phase A;

[0039] Step 2, preparing a composite ethanol solution of zinc chloride, antimony chloride and tin chloride, wherein the concentration of zinc chloride is 12 g / L, the concentration of antimony chloride is 10 g / L, the concentration of tin chloride is 4 g / L, and the solvent is ethanol; soaking the solid phase A in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride, standing for 5 min, then separating the solid and liquid, drying the solid phase at 100 ° C for 10 min, and then calcining at 520 ° C for 15 min; then air cooling to room temperature, soaking in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride again and standing for 5 min, then separating the solid and liquid, drying the solid phase at 100 ° C for 10 min, and then calcining at 520 ° C for 15 min; repeating the above soaking, solid-liquid separation, drying, and calcination process for a total of 10 groups, calcining for the last time for 1 hour, and then air cooling to room temperature to obtain solid phase B;

[0040] Step 3, preparing an aqueous solution of anhydrous ethanol, wherein the volume fraction of anhydrous ethanol in the aqueous solution of anhydrous ethanol is 50%; adding the solid phase B to the aqueous solution of anhydrous ethanol and stirring to form a suspension, wherein the solid-liquid mass ratio of the solid phase B added to the aqueous solution of anhydrous ethanol is solid phase B / the aqueous solution of anhydrous ethanol=1 / 10; adding isopropyl tri(dioctyl pyrophosphate acyloxy) titanate to the suspension, wherein the added mass of isopropyl tri(dioctyl pyrophosphate acyloxy) titanate is 6% of the mass of the solid phase B; after the addition is completed, the suspension is heated to 55±5°C in a water bath, stirred at 60r / min for 1h, then filtered, and dried at 60°C to obtain a solid phase C;

[0041] Step 4: Disperse the solid phase C in ethanol to form an alcohol suspension, the solid-liquid mass ratio of the solid phase C dispersed in ethanol is solid phase C / ethanol=1:20; add coupling agent KH-550 to the alcohol suspension under 60r / min stirring, and the added mass of coupling agent KH-550 is 30% of the mass of the solid phase C; after the addition is completed, continue stirring at 60r / min for 10h, separate the solid and liquid, wash the solid phase with deionized water, dry it, obtain solid phase D, disperse the solid phase D in ethanol solution to obtain an alcohol mixture, the solid-liquid mass ratio of the solid phase D dispersed in the ethanol solution is solid phase D / ethanol=1:20; place the alcohol mixture in a nitrogen atmosphere, keep the water bath temperature at 80±5°C, and then add potassium ethyl xanthate to the alcohol mixture, the added mass of potassium ethyl xanthate is 1% of the mass of the solid phase D. .8 times; after the addition is completed, continue to stir at a constant temperature of 80±5℃ and 60r / min for 12h in a nitrogen atmosphere, then air-cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry; the dried solid phase is dispersed in N,N-dimethylformamide, and the solid-liquid mass ratio of the solid phase dispersed in N,N-dimethylformamide is solid / liquid=1:20; then keep the temperature in a water bath at 60±5℃ in a nitrogen atmosphere, and then add methyl methacrylate and azobisisobutyronitrile in sequence, the mass ratio of the added mass of methyl methacrylate and azobisisobutyronitrile to the solid phase D is methyl methacrylate: azobisisobutyronitrile: solid phase D=3:0.01:1; after the addition is completed, keep warm at 60±5℃ in a nitrogen atmosphere for 12h, then air-cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry to obtain the modified cerium dioxide powder.

[0042] Example 3

[0043] A method for preparing an environmentally friendly high-strength and high-wear-resistant cable material for manufacturing a cable sheath comprises the following steps:

[0044] (1) Weighing the components of the cable material, the components include polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; the weight percentage of each component is as follows: polyvinyl chloride resin 100 parts, nano-attapulgite 18 parts, dioctyl cyclohexane-1,2-dicarboxylate 18 parts, trioctyl phosphite 14 parts, nitrile rubber powder 30 parts, alumina powder 14 parts, light calcium carbonate powder 12 parts, modified cerium dioxide powder 18 parts, zinc borate 8 parts, dilauryl thiodipropionate 0.7 parts, 2,6-di-tert-butyl-4-methylphenol 2 parts, vinyl trimethoxysilane 7 parts, antioxidant TPPD 5 parts, wollastonite powder 12 parts, stearic acid 4 parts;

[0045] (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A;

[0046] (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, stirring evenly after the addition is completed to obtain a mixture B;

[0047] (4) The mixture B is kneaded at a temperature of 105±5°C for 8 minutes, and then mixed and granulated in an extruder at an extrusion temperature of 170°C to obtain a finished cable material. During the cable manufacturing process, the finished cable material is made into a sheath to obtain the environmentally friendly high-strength and high-wear-resistant cable.

[0048] Wherein, the preparation method of the modified cerium dioxide powder is:

[0049] Step 1, preparing an aqueous solution of cerium nitrate and ethylene glycol, wherein the concentration of cerium nitrate is 4g / 100mL and the volume fraction of ethylene glycol is 50%; placing the aqueous solution of cerium nitrate and ethylene glycol in a reactor and keeping the temperature at 65±5°C in a water bath, then stirring the aqueous solution of cerium nitrate and ethylene glycol at 50r / min, and dropping ammonia water into the solution during the stirring process until no precipitation is generated, wherein the mass percentage of the solute in the ammonia water is 25%; then closing the reactor, heating to 120±5°C and keeping the temperature for 4h, air cooling to room temperature after the insulation is completed, opening the reactor, separating the solid and liquid, washing the solid phase with ethanol, and drying to obtain a solid phase A;

[0050] Step 2, preparing a composite ethanol solution of zinc chloride, antimony chloride and tin chloride, wherein the concentration of zinc chloride is 14 g / L, the concentration of antimony chloride is 10 g / L, the concentration of tin chloride is 4 g / L, and the solvent is ethanol; soaking the solid phase A in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride, standing for 5 min, then separating the solid and liquid, drying the solid phase at 100 ° C for 10 min, and then calcining at 520 ° C for 15 min; then air cooling to room temperature, soaking in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride again and standing for 5 min, then separating the solid and liquid, drying the solid phase at 100 ° C for 10 min, and then calcining at 520 ° C for 15 min; repeating the above soaking, solid-liquid separation, drying, and calcination process for a total of 10 groups, calcining for the last time for 1 hour, and then air cooling to room temperature to obtain solid phase B;

[0051] Step 3, preparing an aqueous solution of anhydrous ethanol, wherein the volume fraction of anhydrous ethanol in the aqueous solution of anhydrous ethanol is 50%; adding the solid phase B to the aqueous solution of anhydrous ethanol and stirring to form a suspension, wherein the solid-liquid mass ratio of the solid phase B added to the aqueous solution of anhydrous ethanol is solid phase B / the aqueous solution of anhydrous ethanol=1 / 10; adding isopropyl tri(dioctyl pyrophosphate acyloxy) titanate to the suspension, wherein the added mass of isopropyl tri(dioctyl pyrophosphate acyloxy) titanate is 7% of the mass of the solid phase B; after the addition is completed, the suspension is heated to 55±5°C in a water bath, stirred at 60r / min for 1h, then filtered, and dried at 60°C to obtain a solid phase C;

[0052] Step 4: Disperse the solid phase C in ethanol to form an alcohol suspension, the solid-liquid mass ratio of the solid phase C dispersed in ethanol is solid phase C / ethanol=1:20; add coupling agent KH-550 to the alcohol suspension under 60r / min stirring state, and the added mass of coupling agent KH-550 is 40% of the mass of the solid phase C; after the addition is completed, continue stirring at 60r / min for 10h, separate the solid and liquid, wash the solid phase with deionized water, dry it, obtain solid phase D, and disperse the solid phase D in ethanol solution to obtain an alcohol mixture, the solid-liquid mass ratio of the solid phase D dispersed in the ethanol solution is solid phase D / ethanol=1:20; place the alcohol mixture in a nitrogen atmosphere, keep the water bath temperature at 80±5°C, and then add potassium ethyl xanthate to the alcohol mixture, the added mass of potassium ethyl xanthate is 1% of the mass of the solid phase D. .8 times; after the addition is completed, continue to stir at a constant temperature of 80±5℃ and 60r / min for 12h in a nitrogen atmosphere, then air-cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry; the dried solid phase is dispersed in N,N-dimethylformamide, and the solid-liquid mass ratio of the solid phase dispersed in N,N-dimethylformamide is solid / liquid=1:20; then keep the temperature in a water bath at 60±5℃ in a nitrogen atmosphere, and then add methyl methacrylate and azobisisobutyronitrile in sequence, the mass ratio of the added mass of methyl methacrylate and azobisisobutyronitrile to the solid phase D is methyl methacrylate: azobisisobutyronitrile: solid phase D=4:0.02:1; after the addition is completed, keep warm at 60±5℃ in a nitrogen atmosphere for 12h, then air-cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry to obtain the modified cerium dioxide powder.

[0053] Example 4

[0054] A method for preparing an environmentally friendly high-strength and high-wear-resistant cable material for manufacturing a cable sheath comprises the following steps:

[0055] (1) Weighing the components of the cable material, the components include polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; each component is calculated by weight The invention comprises: 100 parts of polyvinyl chloride resin, 20 parts of nano-attapulgite, 20 parts of dioctyl cyclohexane-1,2-dicarboxylate, 15 parts of trioctyl phosphite, 35 parts of nitrile rubber powder, 16 parts of alumina powder, 13 parts of light calcium carbonate powder, 20 parts of modified cerium dioxide powder, 10 parts of zinc borate, 0.8 parts of dilauryl thiodipropionate, 2 parts of 2,6-di-tert-butyl-4-methylphenol, 9 parts of vinyl trimethoxysilane, 6 parts of antioxidant TPPD, 14 parts of wollastonite powder and 5 parts of stearic acid;

[0056] (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A;

[0057] (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, stirring evenly after the addition is completed to obtain a mixture B;

[0058] (4) The mixture B is kneaded at a temperature of 105±5°C for 8 minutes, and then mixed and granulated in an extruder at an extrusion temperature of 170°C to obtain a finished cable material. During the cable manufacturing process, the finished cable material is made into a sheath to obtain the environmentally friendly high-strength and high-wear-resistant cable.

[0059] Wherein, the preparation method of the modified cerium dioxide powder is:

[0060] Step 1, preparing an aqueous solution of cerium nitrate and ethylene glycol, wherein the concentration of cerium nitrate is 5g / 100mL and the volume fraction of ethylene glycol is 50%; placing the aqueous solution of cerium nitrate and ethylene glycol in a reactor and keeping the temperature at 65±5°C in a water bath, then stirring the aqueous solution of cerium nitrate and ethylene glycol at 50r / min, and adding ammonia water dropwise to the solution during the stirring process until no precipitation is generated, wherein the mass percentage of the solute in the ammonia water is 25%; then closing the reactor, heating to 120±5°C and keeping the temperature for 4h, air cooling to room temperature after the end of the keeping temperature, opening the reactor, separating the solid and liquid, washing the solid phase with ethanol, and drying to obtain a solid phase A;

[0061] Step 2, preparing a composite ethanol solution of zinc chloride, antimony chloride and tin chloride, wherein the concentration of zinc chloride is 16 g / L, the concentration of antimony chloride is 12 g / L, the concentration of tin chloride is 5 g / L, and the solvent is ethanol; soaking the solid phase A in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride, standing for 5 min, then separating the solid and liquid, drying the solid phase at 100 ° C for 10 min, and then calcining at 520 ° C for 15 min; then air cooling to room temperature, soaking in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride again and standing for 5 min, then separating the solid and liquid, drying the solid phase at 100 ° C for 10 min, and then calcining at 520 ° C for 15 min; repeating the above soaking, solid-liquid separation, drying, and calcination process for a total of 10 groups, calcining for the last time for 1 hour, and then air cooling to room temperature to obtain solid phase B;

[0062] Step 3, preparing an aqueous solution of anhydrous ethanol, wherein the volume fraction of anhydrous ethanol in the aqueous solution of anhydrous ethanol is 50%; adding the solid phase B to the aqueous solution of anhydrous ethanol and stirring to form a suspension, wherein the solid-liquid mass ratio of the solid phase B added to the aqueous solution of anhydrous ethanol is solid phase B / the aqueous solution of anhydrous ethanol=1 / 10; adding isopropyl tri(dioctyl pyrophosphate acyloxy) titanate to the suspension, wherein the added mass of isopropyl tri(dioctyl pyrophosphate acyloxy) titanate is 8% of the mass of the solid phase B; after the addition is completed, the suspension is heated to 55±5°C in a water bath, stirred at 60r / min for 1h, then filtered, and dried at 60°C to obtain a solid phase C;

[0063] Step 4: Disperse the solid phase C in ethanol to form an alcohol suspension, the solid-liquid mass ratio of the solid phase C dispersed in ethanol is solid phase C / ethanol = 1:20; add coupling agent KH-550 to the alcohol suspension under 60r / min stirring, and the added mass of coupling agent KH-550 is 40% of the mass of the solid phase C; after the addition is completed, continue stirring at 60r / min for 10h, separate the solid and liquid, wash the solid phase with deionized water, dry it, and obtain solid phase D, disperse the solid phase D in ethanol solution to obtain an alcohol mixture, the solid-liquid mass ratio of the solid phase D dispersed in the ethanol solution is solid phase D / ethanol = 1:20; place the alcohol mixture in a nitrogen atmosphere, keep the water bath temperature at 80±5°C, and then add potassium ethyl xanthate to the alcohol mixture, and the added mass of potassium ethyl xanthate is 2% of the mass of the solid phase D. .0 times; after the addition is completed, continue to stir at a constant temperature of 80±5℃ and 60r / min for 12h in a nitrogen atmosphere, then air-cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry; the dried solid phase is dispersed in N,N-dimethylformamide, and the solid-liquid mass ratio of the solid phase dispersed in N,N-dimethylformamide is solid / liquid=1:20; then keep the temperature in a water bath at 60±5℃ in a nitrogen atmosphere, and then add methyl methacrylate and azobisisobutyronitrile in sequence, the mass ratio of the added mass of methyl methacrylate and azobisisobutyronitrile to the solid phase D is methyl methacrylate: azobisisobutyronitrile: solid phase D=4:0.02:1; after the addition is completed, keep warm at 60±5℃ in a nitrogen atmosphere for 12h, then air-cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry to obtain the modified cerium dioxide powder.

[0064] Comparative Example 1

[0065] A method for preparing a cable material for comparison comprises the following steps:

[0066] (1) Weighing the components of the cable material, the components include polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; the components are calculated by weight as follows: 100 parts of polyvinyl chloride resin, 18 parts of nano-attapulgite, 18 parts of dioctyl cyclohexane-1,2-dicarboxylate, 14 parts of trioctyl phosphite, 30 parts of nitrile rubber powder, 14 parts of alumina powder, 12 parts of light calcium carbonate powder, 8 parts of zinc borate, 0.7 parts of dilauryl thiodipropionate, 2 parts of 2,6-di-tert-butyl-4-methylphenol, 7 parts of vinyl trimethoxysilane, antioxidant TPPD 5 parts, wollastonite powder 12 parts, stearic acid 4 parts;

[0067] (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A;

[0068] (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, and stirring evenly after the addition to obtain a mixture B;

[0069] (4) The mixture B was kneaded at 105±5° C. for 8 min, and then mixed and granulated in an extruder at an extrusion temperature of 170° C. to obtain the finished cable material of this comparative example.

[0070] Comparative Example 2

[0071] A method for preparing a cable material for comparison comprises the following steps:

[0072] (1) Weighing the components of the cable material, the components include polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; each component is calculated by weight The invention comprises: 100 parts of polyvinyl chloride resin, 18 parts of nano-attapulgite, 18 parts of dioctyl cyclohexane-1,2-dicarboxylate, 14 parts of trioctyl phosphite, 30 parts of nitrile rubber powder, 14 parts of alumina powder, 12 parts of light calcium carbonate powder, 18 parts of cerium dioxide powder, 8 parts of zinc borate, 0.7 parts of dilauryl thiodipropionate, 2 parts of 2,6-di-tert-butyl-4-methylphenol, 7 parts of vinyl trimethoxysilane, 5 parts of antioxidant TPPD, 12 parts of wollastonite powder and 4 parts of stearic acid;

[0073] (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A;

[0074] (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, and stirring evenly after the addition to obtain a mixture B;

[0075] (4) The mixture B was kneaded at 105±5° C. for 8 min, and then mixed and granulated in an extruder at an extrusion temperature of 170° C. to obtain the finished cable material of this comparative example.

[0076] The preparation method of the cerium dioxide powder is as follows: prepare an aqueous solution of cerium nitrate and ethylene glycol, wherein the concentration of cerium nitrate is 4g / 100mL and the volume fraction of ethylene glycol is 50%; place the aqueous solution of cerium nitrate and ethylene glycol in a reactor and keep the temperature at 65±5°C in a water bath, then stir the aqueous solution of cerium nitrate and ethylene glycol at 50r / min, and add ammonia water dropwise to the solution during the stirring process until no precipitation is generated, wherein the mass percentage of the solute in the ammonia water is 25%; then close the reactor, heat to 120±5°C and keep warm for 4h, air cool to room temperature after the insulation is completed, open the reactor, separate the solid and liquid, wash the solid phase with ethanol, and dry to obtain the cerium dioxide powder described in this comparative example.

[0077] Comparative Example 3

[0078] A method for preparing a cable material for comparison comprises the following steps:

[0079] (1) Weighing the components of the cable material, the components include polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; each component is calculated by weight The invention comprises: 100 parts of polyvinyl chloride resin, 18 parts of nano-attapulgite, 18 parts of dioctyl cyclohexane-1,2-dicarboxylate, 14 parts of trioctyl phosphite, 30 parts of nitrile rubber powder, 14 parts of alumina powder, 12 parts of light calcium carbonate powder, 18 parts of modified cerium dioxide powder, 8 parts of zinc borate, 0.7 parts of dilauryl thiodipropionate, 2 parts of 2,6-di-tert-butyl-4-methylphenol, 7 parts of vinyl trimethoxysilane, 5 parts of antioxidant TPPD, 12 parts of wollastonite powder and 4 parts of stearic acid;

[0080] (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A;

[0081] (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, stirring evenly after the addition is completed to obtain a mixture B;

[0082] (4) The mixture B was kneaded at 105±5° C. for 8 min, and then mixed and granulated in an extruder at an extrusion temperature of 170° C. to obtain the finished cable material of this comparative example.

[0083] Wherein, the preparation method of the modified cerium dioxide powder is:

[0084] Step 1, preparing an aqueous solution of cerium nitrate and ethylene glycol, wherein the concentration of cerium nitrate is 4g / 100mL and the volume fraction of ethylene glycol is 50%; placing the aqueous solution of cerium nitrate and ethylene glycol in a reactor and keeping the temperature at 65±5°C in a water bath, then stirring the aqueous solution of cerium nitrate and ethylene glycol at 50r / min, and dropping ammonia water into the solution during the stirring process until no precipitation is generated, wherein the mass percentage of the solute in the ammonia water is 25%; then closing the reactor, heating to 120±5°C and keeping the temperature for 4h, air cooling to room temperature after the insulation is completed, opening the reactor, separating the solid and liquid, washing the solid phase with ethanol, and drying to obtain a solid phase A;

[0085] Step 2, prepare an aqueous solution of anhydrous ethanol, wherein the volume fraction of anhydrous ethanol in the aqueous solution of anhydrous ethanol is 50%; add the solid phase A to the aqueous solution of anhydrous ethanol and stir to form a suspension, wherein the solid-liquid mass ratio of the solid phase A added to the aqueous solution of anhydrous ethanol is solid phase A / the aqueous solution of anhydrous ethanol=1 / 10; add isopropyl tri(dioctyl pyrophosphate acyloxy) titanate to the suspension, wherein the added mass of isopropyl tri(dioctyl pyrophosphate acyloxy) titanate is 7% of the mass of the solid phase A; after the addition is completed, the suspension is heated to 55±5°C in a water bath, stirred at 60r / min for 1h, then filtered, and dried at 60°C to obtain the solid phase C described in this comparative example;

[0086] Step 3, dispersing the solid phase C in ethanol to form an alcohol suspension, the solid-liquid mass ratio of the solid phase C dispersed in ethanol is solid phase C / ethanol = 1:20; adding coupling agent KH-550 to the alcohol suspension under 60r / min stirring state, the added mass of coupling agent KH-550 is 40% of the mass of the solid phase C; after the addition is completed, continue stirring at 60r / min for 10h, separate the solid and liquid, wash the solid phase with deionized water, dry to obtain solid phase D, disperse the solid phase D in ethanol solution to obtain an alcohol mixture, the solid-liquid mass ratio of the solid phase D dispersed in the ethanol solution is solid phase D / ethanol = 1:20; placing the alcohol mixture in a nitrogen atmosphere, keeping the water bath temperature at 80±5°C, and then adding potassium ethyl xanthate to the alcohol mixture, the added mass of potassium ethyl xanthate is 1.8 of the mass of the solid phase D times; after the addition is completed, continue to stir at a constant temperature of 80±5℃ and 60r / min in a nitrogen atmosphere for 12h, then air cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry; the dried solid phase is dispersed in N,N-dimethylformamide, and the solid-liquid mass ratio of the solid phase dispersed in N,N-dimethylformamide is solid / liquid=1:20; then keep the temperature in a water bath at 60±5℃ in a nitrogen atmosphere, and then add methyl methacrylate and azobisisobutyronitrile in sequence, the mass ratio of the added mass of the methyl methacrylate and azobisisobutyronitrile to the solid phase D is methyl methacrylate: azobisisobutyronitrile: solid phase D=4:0.02:1; after the addition is completed, keep warm at 60±5℃ in a nitrogen atmosphere for 12h, then air cool to room temperature, separate the solid and liquid, wash the solid phase with ethanol, and dry to obtain the modified cerium dioxide powder described in this comparative example.

[0087] Comparative Example 4

[0088] A method for preparing a cable material for comparison comprises the following steps:

[0089] (1) Weighing the components of the cable material, the components include polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; each component is calculated by weight The invention comprises: 100 parts of polyvinyl chloride resin, 18 parts of nano-attapulgite, 18 parts of dioctyl cyclohexane-1,2-dicarboxylate, 14 parts of trioctyl phosphite, 30 parts of nitrile rubber powder, 14 parts of alumina powder, 12 parts of light calcium carbonate powder, 18 parts of modified cerium dioxide powder, 8 parts of zinc borate, 0.7 parts of dilauryl thiodipropionate, 2 parts of 2,6-di-tert-butyl-4-methylphenol, 7 parts of vinyl trimethoxysilane, 5 parts of antioxidant TPPD, 12 parts of wollastonite powder and 4 parts of stearic acid;

[0090] (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A;

[0091] (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, stirring evenly after the addition is completed to obtain a mixture B;

[0092] (4) The mixture B was kneaded at 105±5° C. for 8 min, and then mixed and granulated in an extruder at an extrusion temperature of 170° C. to obtain the finished cable material of this comparative example.

[0093] Wherein, the preparation method of the modified cerium dioxide powder is:

[0094] Step 1, preparing an aqueous solution of cerium nitrate and ethylene glycol, wherein the concentration of cerium nitrate is 4g / 100mL and the volume fraction of ethylene glycol is 50%; placing the aqueous solution of cerium nitrate and ethylene glycol in a reactor and keeping the temperature at 65±5°C in a water bath, then stirring the aqueous solution of cerium nitrate and ethylene glycol at 50r / min, and dropping ammonia water into the solution during the stirring process until no precipitation is generated, wherein the mass percentage of the solute in the ammonia water is 25%; then closing the reactor, heating to 120±5°C and keeping the temperature for 4h, air cooling to room temperature after the insulation is completed, opening the reactor, separating the solid and liquid, washing the solid phase with ethanol, and drying to obtain a solid phase A;

[0095] Step 2, preparing a composite ethanol solution of zinc chloride, antimony chloride and tin chloride, wherein the concentration of zinc chloride is 14 g / L, the concentration of antimony chloride is 10 g / L, the concentration of tin chloride is 4 g / L, and the solvent is ethanol; soaking the solid phase A in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride, standing for 5 min, then separating the solid and liquid, drying the solid phase at 100 ° C for 10 min, and then calcining at 520 ° C for 15 min; then air cooling to room temperature, soaking in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride again and standing for 5 min, then separating the solid and liquid, drying the solid phase at 100 ° C for 10 min, and then calcining at 520 ° C for 15 min; repeating the above soaking, solid-liquid separation, drying, and calcination process for a total of 10 groups, calcining for the last time for 1 hour, and then air cooling to room temperature to obtain solid phase B;

[0096] Step 3, prepare an aqueous solution of anhydrous ethanol, in which the volume fraction of anhydrous ethanol is 50%; add the solid phase B to the aqueous solution of anhydrous ethanol and stir to form a suspension, the solid-liquid mass ratio of the solid phase B added to the aqueous solution of anhydrous ethanol is solid phase B / anhydrous ethanol aqueous solution=1 / 10; add isopropyl tri(dioctyl pyrophosphate) titanate to the suspension, and the added mass of isopropyl tri(dioctyl pyrophosphate) titanate is 7% of the mass of solid phase B; after the addition is completed, the suspension is kept at a constant temperature of 55±5°C in a water bath, stirred at 60r / min for 1h, then filtered, and dried at 60°C to obtain the modified cerium dioxide powder described in this comparative example.

[0097] Example 5

[0098] The cable materials obtained by the methods described in the above embodiments and comparative examples were respectively prepared into standard specimens specified in various test standards according to the national standard GB / T8815-2008, and the material properties of the specimens were tested according to the requirements of the national standard GB / T 8815-2008. The tensile strength and low-temperature brittle temperature results are shown in Table 1.

[0099] As shown in Table 1, the cable material prepared by the method of the present invention has good mechanical properties and low temperature resistance, which is manifested as high tensile strength and low temperature brittle temperature, and is suitable for manufacturing wires and cables with high strength requirements, and can also be used to manufacture cables that work in low temperature environments for a long time, and has a wide range of applications. Comparative Example 3 and each comparative example show that on the basis of the cable material formula of the present application, after adding modified cerium dioxide powder, the tensile strength and low temperature brittle temperature are significantly improved, which may be caused by the strengthening effect of the second phase of cerium dioxide, and then through the modification of cerium dioxide in the present application, the dispersibility of cerium dioxide in the matrix material and the wettability of the dispersed cerium dioxide particles and the matrix are improved, so that the mechanical properties and low temperature properties of the cable material are optimized macroscopically.

[0100] Table 1

[0101] Experimental Group Tensile strength(MPa) Low temperature brittleness temperature (℃) Example 1 22.8 -68 Example 2 23.2 -71 Example 3 23.4 -73 Example 4 23.7 -70 Comparative Example 1 14.5 -36 Comparative Example 2 16.9 -41 Comparative Example 3 20.1 -59 Comparative Example 4 19.3 -52

[0102] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for preparing an environmentally friendly high-strength and high-wear-resistant cable, characterized in that: The steps include: (1) Weigh the components of the cable material, which include polyvinyl chloride resin, nano-attapulgite, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid; the weight proportion of each component is as follows: 100 parts of polyvinyl chloride resin, 100 parts of nano-attapulgite, 100 parts of cyclohexane-1,2-dicarboxylate, trioctyl phosphite, nitrile rubber powder, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid. 10-20 parts of attapulgite, 15-20 parts of dioctyl cyclohexane-1,2-dicarboxylate, 10-15 parts of trioctyl phosphite, 25-35 parts of nitrile rubber powder, 10-16 parts of alumina powder, 10-13 parts of light calcium carbonate powder, 12-20 parts of modified cerium dioxide powder, 5-10 parts of zinc borate, 0.5-0.8 parts of dilauryl thiodipropionate, 1-2 parts of 2,6-di-tert-butyl-4-methylphenol, 5-9 parts of vinyl trimethoxysilane, 3-6 parts of antioxidant TPPD, 10-14 parts of wollastonite powder, and 2-5 parts of stearic acid; (2) mixing polyvinyl chloride resin, dioctyl cyclohexane-1,2-dicarboxylate, trioctyl phosphite and nitrile rubber powder in a mixer at a temperature range of 50±5° C. to obtain a mixture A; (3) raising the temperature of the mixture A to 75±5° C., then adding nano-attapulgite, alumina powder, light calcium carbonate powder, modified cerium dioxide powder, zinc borate, dilauryl thiodipropionate, 2,6-di-tert-butyl-4-methylphenol, vinyl trimethoxysilane, antioxidant TPPD, wollastonite powder and stearic acid to the mixture A, and stirring evenly after the addition to obtain a mixture B; (4) kneading the mixture B at a temperature of 100 to 110° C. for 7 to 10 minutes, and then kneading and granulating in an extruder at an extrusion temperature of 150 to 180° C. to obtain a finished cable material. In the cable manufacturing process, the finished cable material is made into a sheath to obtain the environmentally friendly high-strength and high-wear-resistant cable; Wherein, the preparation method of the modified cerium dioxide powder is: Step 1, preparing an aqueous solution of cerium nitrate and ethylene glycol, placing the aqueous solution of cerium nitrate and ethylene glycol in a reactor and keeping the temperature at 65±5°C in a water bath, then stirring the aqueous solution of cerium nitrate and ethylene glycol, and dropping ammonia water into the solution during the stirring process until no precipitation is generated, then sealing the reactor, heating to 120±5°C and keeping the temperature for 4-5h, air cooling to room temperature after the insulation is completed, opening the reactor, separating the solid and liquid, washing the solid phase with ethanol, and drying to obtain a solid phase A; Step 2: prepare a composite ethanol solution of zinc chloride, antimony chloride and tin chloride, immerse the solid phase A in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride, let it stand for 5 to 6 minutes, then separate the solid and liquid, dry the solid phase at 100 to 120° C. for more than 10 minutes, and then calcine at 500 to 550° C. for more than 15 minutes; then air-cool to room temperature, immerse it in the composite ethanol solution of zinc chloride, antimony chloride and tin chloride again and let it stand for 5 to 6 minutes, then separate the solid and liquid, dry the solid phase at 100 to 120° C. for more than 10 minutes, and then calcine at 500 to 550° C. for more than 15 minutes; repeat the above immersion, solid-liquid separation, drying and calcination process for a total of 10 to 12 groups, calcine for the last time for 1 to 2 hours, and then air-cool to room temperature to obtain solid phase B; Step 3: prepare an aqueous solution of anhydrous ethanol, add the solid phase B to the aqueous solution of anhydrous ethanol and stir to form a suspension, add isopropyl tri(dioctyl pyrophosphate acyloxy) titanate to the suspension, and after the addition is completed, keep the suspension in a water bath at a constant temperature of 55±5°C, keep it warm and stir for more than 1h, then filter it, and dry it at 60°C to obtain a solid phase C; Step 4: Disperse the solid phase C in ethanol to form an alcohol suspension, add coupling agent KH-550 to the alcohol suspension under stirring, continue stirring for more than 10 hours after the addition is completed, separate the solid and liquid, wash the solid phase with deionized water, dry it, and obtain a solid phase D, disperse the solid phase D in an ethanol solution to obtain an alcohol mixture, place the alcohol mixture in a nitrogen atmosphere, keep the water bath temperature at 80±5°C, then add potassium ethyl xanthate to the alcohol mixture, and continue to stir under nitrogen after the addition is completed. The mixture is stirred at a constant temperature of 80±5°C in an atmosphere for more than 12 hours, then air-cooled to room temperature, the solid-liquid is separated, the solid phase is washed with ethanol, and dried; the dried solid phase is dispersed in N,N-dimethylformamide, and then the temperature is kept constant at 60±5°C in a water bath in a nitrogen atmosphere, and methyl methacrylate and azobisisobutyronitrile are added in sequence. After the addition is completed, the mixture is kept warm at 60±5°C in a nitrogen atmosphere for more than 12 hours, then air-cooled to room temperature, the solid-liquid is separated, the solid phase is washed with ethanol, and dried to obtain the modified cerium dioxide powder.

2. The method for preparing an environmentally friendly high-strength and high-wear-resistant cable according to claim 1, characterized in that: In the aqueous solution of cerium nitrate and ethylene glycol, the concentration of cerium nitrate is 3-5 g / 100 mL, the volume fraction of ethylene glycol is 50%, and the mass percentage of the solute in the ammonia water is 25%.

3. The method for preparing an environmentally friendly high-strength and high-wear-resistant cable according to claim 1, characterized in that: In the composite ethanol solution of zinc chloride, antimony chloride and tin chloride, the concentration of zinc chloride is 10-16 g / L, the concentration of antimony chloride is 8-12 g / L, the concentration of tin chloride is 3-5 g / L, and the solvent is ethanol.

4. The method for preparing an environmentally friendly high-strength and high-wear-resistant cable according to claim 1, characterized in that: In the step 3, the volume fraction of anhydrous ethanol in the aqueous solution of anhydrous ethanol is 50%; the solid-liquid mass ratio of the solid phase B added to the aqueous solution of anhydrous ethanol is solid phase B / anhydrous ethanol aqueous solution=1 / 10, and the added mass of the isopropyl tri(dioctyl pyrophosphate) titanate is 5% to 8% of the mass of the solid phase B.

5. The method for preparing an environmentally friendly high-strength and high-wear-resistant cable according to claim 1, characterized in that: In the step 4, the solid-liquid mass ratio of the solid phase C dispersed in ethanol is solid phase C / ethanol=1:20; the added mass of the coupling agent KH-550 is 30% to 40% of the mass of the solid phase C; the solid-liquid mass ratio of the solid phase D dispersed in the ethanol solution is solid phase D / ethanol=1:20; the added mass of the potassium ethyl xanthate is 1.6 to 2.0 times the mass of the solid phase D; the solid-liquid mass ratio of the dried solid phase dispersed in N,N-dimethylformamide is solid / liquid=1:20; the mass ratio of the added mass of methyl methacrylate and azobisisobutyronitrile to the solid phase D is methyl methacrylate: azobisisobutyronitrile: solid phase D=3 to 4:0.01 to 0.02:1.