A method for producing hull steel with good plate shape by using CSP
By using the CSP method in marine steel production, the chemical composition and process steps are controlled, and the problem of poor plate-shaped control ability of thin specification high-strength steel is solved, and the production of hull steel with high strength, high toughness and good plate-shaped quality is achieved. Meet the classification societies standards and reduce production costs.
Patent Information
- Application Number
- CN202310175745.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-02-28
AI Technical Summary
In the production of marine steel, the plate-shaped control capability of thin specifications and high-strength steels has poor rolling stability and temperature uniformity problems, affecting the dimensional accuracy and plate-shaped quality of the product, and the cost of material alloys is high, and the difficulty of smelting is Increase.
Using CSP production method, the chemical compositions were controlled as C: 0.03-0.065%, Si: ≤0.20%, Mn: 0.80-1.00%, P: ≤0.020%, S: ≤0.012%, Als: 0.015-0.055%, Ti: 0.020~0.040%, N: ≤0.008%, ensure that the process steps such as iron desulfurization, converter steelmaking, LF furnace refining, RH vacuum treatment, casting into blanks, heat treatment, equal proportional convex rolling and fast cooling in the front section are ensured. The plate-shaped quality of steel.
The hull steel with a thickness specification of 2 to 8mm was realized, with yield strength ≥350MPa, tensile strength ≥470MPa, elongation after break A≥27%, impact work Akv≥105J in 0℃, meeting the material mechanical properties and plates of the classification society Measure quality standards and reduce production costs by at least 5%.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to a steel for ship engineering and a production method thereof, and in particular to a hull steel with good plate shape produced by adopting CSP and a production method thereof. Background Art
[0002] The construction of a steel hull is a complex production process. Marine steel materials are pre-treated, then cut, welded, and formed into parts, and then assembled into components, various sections (planes, curved surfaces, etc.), and total sections. Finally, they are welded and assembled on the slipway or dock until the entire hull is formed. According to the processing characteristics of the shipbuilding industry, marine steel is required to have good toughness and welding performance under certain strength conditions, and have good dimensional accuracy and plate quality. Reducing the weight and increasing the load of ships has become the goal of major shipbuilding companies, and high-strength thinning of marine steel has become an inevitable choice. When thin-gauge high-strength marine steel is produced on the hot rolling production line, due to the long production line, fast temperature drop and poor temperature uniformity control, the rolling load is large, the rolling stability is poor, the plate shape control ability of marine steel is poor, the production efficiency is low, and the product yield rate is low. The CSP production line has advantages due to its short process, low energy consumption, and high production efficiency, especially in the production of thin-gauge products, with high product dimensional accuracy control and good plate shape control. Therefore, the use of CSP technology to produce thin-gauge high-strength marine steel products is an economical and efficient production method, and the products have good dimensional accuracy and excellent plate quality.
[0003] After searching:
[0004] The document with Chinese patent application number CN200710020524.7 records "High-strength steel for ship hull structure and its coil production method". The process route adopted is steelmaking → refining → CSP continuous casting → heating → rolling → cooling → coiling, and the mass percentage of steel is C = 0.03-0.075%, Si = 0.01-0.35%, Mn = 1.40-1.60%, Als = 0.015-0.10%, V = 0.020-0.080%. Due to its high Mn content and the addition of V, it is obvious that not only the material alloy cost is increased, but also the difficulty of smelting is increased. Moreover, the document does not have a clear control method for the material plate shape quality. The material produced by this patented method has plate shape defects in the rolling stage due to the lack of rolling stability and rolling uniformity control method in terms of rolling plate shape control. In the cooling process, since there is no uniformity control method for cooling temperature, cooling plate shape defects will occur. The superposition of the two plate shape defects will lead to plate shape quality defects in the final product.
[0005] The document with Chinese patent publication number CN104962813A records "economical high-strength steel with good formability based on CSP production line and its manufacturing method", and its chemical composition is calculated by weight percentage as C: 0.04-0.07, Si: 0.10-0.30, Mn: 1.20-1.50, P: ≤0.015, S: ≤0.004, Ti: 0.13-0.18, N: ≤0.004, Als: 0.02-0.04, O: ≤0.002, and the rest is Fe and unavoidable inclusions. The steel coil in this document belongs to the field of easy-to-form high-strength structural steel, which is essentially different from ship steel products. Ship steel has specific composition requirements and process performance requirements, and must comply with the relevant standards of the classification society before it can be used as ship steel material. Summary of the invention
[0006] The present invention aims to overcome the shortcomings of the prior art and provide a kind of material with a thickness of 2 to 8 mm, a yield strength of ≥350 MPa, a tensile strength of ≥470 MPa, an elongation after fracture A of ≥27%, and an impact energy Akv of 0°C.
[0007] A hull steel with good plate shape produced by CSP and a production method thereof.
[0008] Measures to achieve the above objectives:
[0009] A hull steel with good plate shape produced by CSP, the components and weight percentage of which are: C: 0.03-0.065%, Si: ≤0.20%, Mn: 0.80-1.00%, P: ≤0.020%, S: ≤0.012%, Als: 0.015-0.055%, Ti: 0.020-0.040%, N: ≤0.008%, and the rest is Fe and unavoidable inclusions.
[0010] Preferably, the weight percentage of Mn is 0.80-0.95%.
[0011] Preferably, the weight percentage content of Ti is 0.020-0.035%.
[0012] A method for producing economical hull steel with good plate shape by using CSP, comprising the following steps:
[0013] 1) Desulfurization of molten iron, and control the S of molten iron after desulfurization to ≤ 0.008%;
[0014] 2) Converter steelmaking, and control the C content in the molten steel to be no less than 0.03% at the end of steelmaking, and the tapping temperature to be between 1650 and 1680°C;
[0015] 3) Carry out LF furnace refining and control the temperature of molten steel leaving the station to be no less than 1640°C;
[0016] 4) Carry out RH vacuum treatment and control the following conditions at the end: N≤0.004%, Als≤0.004% in molten steel
[0017] 0.015~0.055%, tapping temperature is 1560~1580℃;
[0018] 5) Casting into billets, during which the billet drawing speed is controlled at 3.5-3.7 m / min; the second cooling water section adopts the edge weak cooling system, and the cooling water volume is such that the temperature of the slab entering the soaking furnace is 800-1050°C;
[0019] 6) Heat the ingot, control the temperature of the soaking furnace at 1180-1220℃, and control the total soaking time to be no less than 20min; the temperature difference of the same plate is ≤20℃;
[0020] 7) Use equal proportion crown rolling mode for rolling: control the rolling temperature at 1130-1170℃,
[0021] The pass reduction rate and rolling temperature are:
[0022] F1~F3: The reduction rate of each pass is 55~65%, and the rolling temperature is 1110~1170℃;
[0023] The reduction rate of F4 is 25-35%, and the rolling temperature is 980-1100℃;
[0024] F5-F6: The reduction rate of each pass is 10-15%, and the rolling temperature is 920-980℃;
[0025] The reduction rate of F7 is 6-9%, and the rolling temperature is 860-900℃;
[0026] And during the rolling process, it is ensured that the austenite is fully recrystallized;
[0027] 8) The steel plate is cooled to the coiling temperature at a cooling rate of 80-150°C / s; water cooling is performed on the side, and the temperature of the steel plate entering the middle section is controlled at 690-710°C;
[0028] 9) Coil the steel sheet and control the coiling temperature at 610-650°C.
[0029] The functions and mechanisms of various raw materials and main processes in the present invention are described as follows:
[0030] The carbon (C) content of the present invention is 0.030% to 0.065%. Carbon is one of the indispensable elements in steel for improving the strength of steel. Reducing the content can avoid the range of peritectic steel and ensure the stability of thin slab continuous casting. At the same time, in order to ensure a lower carbon equivalent, improve the welding performance of the steel plate and improve its toughness, the carbon content is limited to 0.030% to 0.065%.
[0031] The silicon (Si) content of the present invention is ≤0.20%. Si has a certain solid solution strengthening effect, which is beneficial to improving the strength of the steel but not conducive to the control of toughness. Under high temperature conditions, Si is first oxidized to SiO2, and then SiO2 reacts with FeO in the oxide layer to form fayalite phase Fe2SiO4 (2FeO·SiO2), which is easily enriched at the bonding surface of the iron oxide scale and the substrate, and is not easy to remove, thereby affecting the rolled surface quality. Moreover, if the Si content is too high, micro cracks caused by oxide indentation are easily formed on the surface, which is not conducive to the control of the surface quality of the steel plate. Therefore, the Si content of the present invention is controlled to be ≤0.20%.
[0032] The manganese (Mn) content of the present invention is 0.80% to 1.00%. Manganese is the main solid solution strengthening element and has the effect of significantly refining grains. An appropriate amount of Mn content can reduce the γ→α phase transition temperature, help obtain fine phase transition products, and improve toughness. At the same time, since manganese and sulfur have a large affinity, FeS can be avoided from precipitating at the grain boundary, reducing hot brittleness and improving hot processing performance. However, when the Mn content is higher than 1.0%, (FeMn)2SiO4 is easily generated and easily enriched at the interface between the iron oxide scale and the substrate, causing the roughness of the interface between the iron oxide scale and the substrate, and forming defects such as the iron oxide scale. Therefore, the present invention controls the Mn content to 0.80% to 1.00%, preferably 0.80% to 0.95%.
[0033] The phosphorus (P) content of the present invention is ≤0.020%, and the sulfur (S) content is ≤0.012%. S mainly affects the plasticity of the steel and is easily combined with manganese to form MnS inclusions. P mainly affects the impact toughness and tough-brittle transition temperature of the steel and is easy to cause segregation in the steel. Therefore, the present invention should minimize the adverse effects of phosphorus and sulfur elements, and control the P and S contents of the steel to P: ≤0.020%, S: ≤0.012%.
[0034] The acid-soluble aluminum (Als) content of the present invention is 0.015-0.055%. Als is a main deoxidizing element, which can reduce oxide inclusions in steel, purify steel quality, refine grains, and at the same time, inhibit the aging of low-carbon steel, improve the toughness of steel at low temperatures, especially reduce the brittle transition temperature of steel, and improve the oxidation resistance of steel. Therefore, the Als content of the present invention is in the range of 0.015-0.055%.
[0035] The titanium (Ti) content of the present invention is 0.020-0.040%. Ti has extremely strong binding force with carbon, nitrogen and oxygen, and forms corresponding compounds with them, has excellent hydrogen resistance, improves the strength of steel, improves the welding performance of steel, and increases toughness. However, when the Ti content is lower than the limit value, it cannot achieve the purpose of precipitation strengthening, and only combines with N and S in a limited manner, and cannot generate effective TiC. When the Ti content is higher than the limit value, ferrite δ phase or other brittle phases are easily generated, which reduces the toughness of the material. Therefore, the Ti content of the present invention ranges from 0.020% to 0.040%, preferably from 0.020% to 0.035%.
[0036] The nitrogen (N) content of the present invention is ≤0.008%. The energy of TiN generated by combining with N is very low, and it begins to precipitate in the solidification process of molten steel. The presence of N will seriously reduce the effective Ti content, affecting the precipitation strengthening of TiC. The formed TiN square particles are likely to become the source of cracks during material forming or impact, resulting in material forming cracking problems. Therefore, the N content range of the present invention is ≤0.008%.
[0037] The smelting of the present invention requires pretreatment of molten iron desulfurization S: ≤0.008%; converter molten steel smelting C ≥0.03%, and the tapping temperature is 1650-1680°C; deoxidation and slag making in the LF furnace, the leaving station temperature is ≥1640°C; the molten steel enters the RH furnace for decarburization and deoxidation; calcium treatment is used to improve the slag properties, N is controlled to be ≤0.004%, Als is controlled to be 0.015-0.055%, and the tapping temperature is 1560-1580°C.
[0038] The invention controls the continuous casting billet drawing speed at 3.5-3.7 m / min, adopts the edge weak cooling system in the second cooling water section, controls the cooling water volume to ensure that the temperature of the continuous casting thin slab entering the soaking furnace is 800-1050°C, and reduces the edge cracks of the billet.
[0039] The reason why the soaking time in the furnace is controlled to be ≥20min and the temperature out of the soaking furnace is controlled to be 1180-1220℃ is that the factors affecting the thickness accuracy and plate shape are mainly temperature unevenness and the stability of the roller system. Temperature unevenness will cause changes in rolling force and plasticity coefficient, resulting in thickness deviation and thus causing the steel plate to be stretched to the sides or up and down, so the temperature difference of the same plate is required to be ≤20℃.
[0040] The invention controls the start rolling temperature to 1130-1170°C, adopts the equal proportion crown rolling mode, and the reduction rate and rolling temperature of each pass are respectively: F1-F3: 55-65%, 1110-1170°C; F4: 25-35%, 980-1100°C; F5-F6: 10-15%, 920-980°C; F7: 6-9%, 860-900°C; during the rolling process, the opening of the finishing mill water is strictly controlled to be ≤2, reducing the influence of the mill water on the strip temperature, improving the control of the final rolling temperature, and also improving the uniformity of the temperature of the coil edge. Avoid uneven deformation of the slab due to uneven temperature during the rolling process, thereby generating large uneven deformation resistance, resulting in large uneven deformation stress and thermal stress, and also ensure that the austenite fully recrystallizes, eliminates the mixed crystal defects in the organization, and ensures the quality of the final rolled plate shape.
[0041] The reason why the present invention requires the use of front-end fast cooling, the cooling rate controlled at 80-150°C / s, and the side water spraying is to ensure cooling uniformity, ensure that the intermediate cooling temperature is 690-710°C, and the final coiling temperature is 610-650°C.
[0042] Compared with the prior art, the present invention reduces the dosage of Mn and Ti elements, but can also make the yield strength ≥350MPa, the tensile strength ≥470MPa, the elongation after fracture A ≥27%, and the impact energy A at 0℃ kv ≥105J, thickness specification is 2~8mm, that is, the CSP production line is fully capable of producing steel that meets the high standards of material mechanical properties and plate quality for hull use, and the production cost can be reduced by at least 5% compared with the traditional production line. DETAILED DESCRIPTION
[0043] The present invention is described in detail below:
[0044] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;
[0045] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;
[0046] Table 3 is a table of performance test results of various embodiments of the present invention and comparative examples.
[0047] Each embodiment of the present invention is produced according to the following steps
[0048] 1) Desulfurization of molten iron, and control the S of molten iron after desulfurization to ≤ 0.008%;
[0049] 2) Converter steelmaking, and control the C content in the molten steel to be no less than 0.03% at the end of steelmaking, and the tapping temperature to be between 1650 and 1680°C;
[0050] 3) Carry out LF furnace refining and control the temperature of molten steel leaving the station to be no less than 1640°C;
[0051] 4) Carry out RH vacuum treatment and control the following conditions at the end: N≤0.004%, Als≤0.004% in molten steel
[0052] 0.015~0.055%, tapping temperature is 1560~1580℃;
[0053] 5) Casting into billets, during which the billet drawing speed is controlled at 3.5-3.7 m / min; the second cooling water section adopts the edge weak cooling system, and the cooling water volume is such that the temperature of the slab entering the soaking furnace is 800-1050°C;
[0054] 6) Heat the ingot, control the temperature of the soaking furnace at 1180-1220℃, and control the total soaking time to be no less than 20min; the temperature difference of the same plate is ≤20℃;
[0055] 7) Use equal proportion crown rolling mode for rolling: control the rolling temperature at 1130-1170℃,
[0056] The pass reduction rate and rolling temperature are:
[0057] F1~F3: The reduction rate of each pass is 55~65%, and the rolling temperature is 1110~1170℃;
[0058] The reduction rate of F4 is 25-35%, and the rolling temperature is 980-1100℃;
[0059] F5-F6: The reduction rate of each pass is 10-15%, and the rolling temperature is 920-980℃;
[0060] The reduction rate of F7 is 6-9%, and the rolling temperature is 860-900℃;
[0061] And during the rolling process, it is ensured that the austenite is fully recrystallized;
[0062] 8) Cooling is performed by a front-stage rapid cooling method, where the steel plate is cooled to the coiling temperature at a cooling rate of 80 to 150°C / s; meanwhile, side water spray cooling is performed, and the temperature of the steel plate entering the middle section is controlled at 690 to 710°C; 9) Coiling is performed, and the coiling temperature is controlled at 610 to 650°C.
[0063] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)
[0064]
[0065] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples
[0066]
[0067]
[0068] Table 2
[0069]
[0070] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples
[0071]
[0072]
[0073] It can be seen from Table 3 that the material produced by this method has a yield strength greater than 350MPa, a tensile strength greater than 470MPa, an elongation after fracture A≥27%, and an impact energy A at 0℃. kv ≥105J, which can fully meet the use standard requirements of classification societies. In addition, since this method adopts CSP production line, it not only has a short production process, but also saves energy and is environmentally friendly, reduces costs and has good market prospects and economic benefits.
[0074] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A hull steel with good plate shape produced by CSP, the components and weight percentage contents of which are: C: 0.03-0.065%, Si: 0.082-0.091%, Mn: 0.80-0.931%, P: ≤0.020%, S: ≤0.012%, Als: 0.015-0.055%, Ti: 0.020-0.040%, N: ≤0.008%, and the rest are Fe and unavoidable inclusions; Production method: 1) Desulfurization of molten iron, and control the S of molten iron after desulfurization to ≤ 0.008%; 2) Converter steelmaking, and control the C content of molten steel to not less than 0.03% at the end of steelmaking, and the tapping temperature to be between 1650 and 1680°C; 3) Carry out LF furnace refining and control the temperature of molten steel leaving the station to be no less than 1640℃; 4) Carry out RH vacuum treatment and control the following conditions in the molten steel at the end: N≤0.004%, Als at 0.015~0.055%, and tapping temperature at 1560~1580℃; 5) Casting into billets, during which the billet drawing speed is controlled at 3.5~3.7m / min; the secondary cooling water section adopts the edge weak cooling system, and the cooling water volume is sufficient to make the temperature of the slab entering the soaking furnace at 800~1050℃; 6) Heat the ingot, control the temperature of the soaking furnace at 1188~1213℃, and control the total soaking time at 20~26min; the temperature difference of the same plate is ≤20℃; 7) Use the equal-proportional crown rolling mode for rolling: control the starting rolling temperature at 1130~1170℃, and the reduction rate and rolling temperature of each pass are as follows: F1~F3: The reduction rate of each pass is 55~65%, and the rolling temperature is 1110~1170℃; The reduction rate of F4 is 25~35%, and the rolling temperature is 980~1100℃; F5~F6: The reduction rate of each pass is 10~15%, and the rolling temperature is 920~980℃; The reduction rate of F7 is 6~9%, and the rolling temperature is 860~900℃; And during the rolling process, ensure that the austenite is fully recrystallized; 8) The steel plate is cooled to the coiling temperature at a cooling rate of 80-150°C / s; water spray cooling is performed on the side, and the temperature of the steel plate entering the middle section is controlled at 690-710°C; 9) Coil the steel sheet and control the coiling temperature at 610~650℃.
2. A method for producing ship hull steel with good plate shape using CSP as claimed in claim 1, comprising the following steps: 1) Desulfurization of molten iron, and control the S of molten iron after desulfurization to ≤ 0.008%; 2) Converter steelmaking, and control the C content of molten steel to not less than 0.03% at the end of steelmaking, and the tapping temperature to be between 1650 and 1680°C; 3) Carry out LF furnace refining and control the temperature of molten steel leaving the station to be no less than 1640℃; 4) Carry out RH vacuum treatment and control the following conditions in the molten steel at the end: N≤0.004%, Als at 0.015~0.055%, and tapping temperature at 1560~1580℃; 5) Casting into billets, during which the billet drawing speed is controlled at 3.5~3.7m / min; the secondary cooling water section adopts the edge weak cooling system, and the cooling water volume is sufficient to make the temperature of the slab entering the soaking furnace at 800~1050℃; 6) Heat the ingot, control the temperature of the soaking furnace at 1188~1213℃, and control the total soaking time at 20~26min; the temperature difference of the same plate is ≤20℃; 7) Use the equal-proportional crown rolling mode for rolling: control the starting rolling temperature at 1130~1170℃, and the reduction rate and rolling temperature of each pass are as follows: F1~F3: The reduction rate of each pass is 55~65%, and the rolling temperature is 1110~1170℃; The reduction rate of F4 is 25~35%, and the rolling temperature is 980~1100℃; F5~F6: The reduction rate of each pass is 10~15%, and the rolling temperature is 920~980℃; The reduction rate of F7 is 6~9%, and the rolling temperature is 860~900℃; And during the rolling process, ensure that the austenite is fully recrystallized; 8) The steel plate is cooled to the coiling temperature at a cooling rate of 80-150°C / s; water spray cooling is performed on the side, and the temperature of the steel plate entering the middle section is controlled at 690-710°C; 9) Coil the steel sheet and control the coiling temperature at 610~650℃.