Fluororesin, laminate, tube, and method for producing tube

By adjusting the loss and storage modulus difference of fluororesin and adding specific units and functional groups, the problems of rough inner surface and uneven thickness of fluororesin in high linear speed extrusion molding are solved, achieving high adhesion and uniformity. properties, improving the quality and productivity of laminated bodies and multi-layer tubes.

CN116234698BActive Publication Date: 2024-10-01DAIKIN INDUSTRIES LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202180063342.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2021-09-30
Publication Date
2024-10-01
Estimated Expiration
2041-09-30

AI Technical Summary

Technical Problem

During the high linear speed extrusion molding process of existing fluororesin, the inner surface of the tube is easily roughened and the thickness is uneven, and the adhesion with other materials is reduced.

Method used

Using specially adjusted fluororesin, the difference in loss modulus between 270℃ and 280℃ (G”270-G”280) is more than 2500Pa, and the difference in storage modulus (G’270-G’280) is more than 1500Pa, and Contains ethylene, tetrafluoroethylene and hexafluoropropylene units with reactive functional groups for forming laminates and tubes with high adhesion.

Benefits of technology

Under high linear speed extrusion molding, the inner surface of the tube is smooth and the thickness is uniform, and the high adhesion to other materials is achieved, which improves the productivity and quality of laminated bodies and multi-layer tubes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004126973050000281
    Figure BDA0004126973050000281
Patent Text Reader

Abstract

Provided is a fluororesin having a reactive functional group, wherein the loss modulus (G" of the fluororesin at 270°C is 270 ) and the loss modulus (G" of the above fluororesin at 280℃ 280 ) difference (G" 270 ‑G" 280 ) is above 2500Pa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a fluororesin, a laminate, a tube, and a method for producing the tube. Background Art

[0002] Tubes made of fluororesins are known. In addition, laminated tubes formed by laminating fluororesins with other polymer materials are also known.

[0003] As a method for manufacturing such a laminated tube, patent document 1 proposes a method for manufacturing a multilayer laminate, which uses a co-extrusion device including a die and a plurality of extruders for supplying resin to the above-mentioned die, and at least polyamide (A) and fluorine-containing olefinic polymer (B) are layered by a simultaneous multi-layer co-extrusion method to obtain a laminate composed of the above-mentioned polyamide (A) and the above-mentioned fluorine-containing olefinic polymer (B). The manufacturing method is characterized in that the temperature of the above-mentioned die is set to a range of more than 260°C and less than 310°C.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2001 / 070485 Summary of the invention

[0007] Problems to be solved by the invention

[0008] An object of the present invention is to provide a fluororesin having high adhesion to other materials and capable of obtaining a tube having a smooth inner surface and a uniform thickness even when the tube is produced by extrusion molding at a high line speed.

[0009] Means for solving problems

[0010] According to the present invention, there is provided a fluororesin having a reactive functional group, wherein the loss modulus (G" of the fluororesin at 270°C is 270 ) and the loss modulus (G”) of the above fluororesin at 280°C 280 ) (G” 270 -G" 280 ) is above 2500Pa.

[0011] The storage modulus (G') of the above fluororesin at 270°C 270 ) and the storage modulus (G') of the above fluororesin at 280°C 280 ) difference (G' 270 -G' 280 ) is preferably above 1500Pa.

[0012] The above-mentioned fluororesin is preferably a melt-processable fluororesin.

[0013] The fluororesin preferably contains ethylene units and tetrafluoroethylene units.

[0014] The above-mentioned fluororesin preferably further contains a hexafluoropropylene unit.

[0015] The number of reactive functional groups of the above fluororesin is relative to every 10 6 The number of carbon atoms in the main chain is preferably 3 or more.

[0016] According to the present invention, there is provided a laminate comprising a fluororesin layer containing the above-mentioned fluororesin and a non-fluororesin layer containing a non-fluororesin.

[0017] As the non-fluorine resin layer, it is preferable to include a polyamide resin layer containing a polyamide resin.

[0018] The fluororesin layer is bonded to the polyamide resin layer, and the interlayer bonding strength between the fluororesin layer and the polyamide resin layer is preferably 30 N / cm or more.

[0019] As the non-fluorine-free resin layer, it is preferable to provide an EVOH layer containing an ethylene / vinyl alcohol copolymer (EVOH) resin.

[0020] Furthermore, according to the present invention, there is provided a multi-layered tube formed of the above-mentioned laminated body.

[0021] Furthermore, according to the present invention, there is provided a single-layer tube comprising the above-mentioned fluororesin.

[0022] The inner surface of the tube is formed of the fluororesin, and the surface roughness Ra of the inner surface is preferably 1.0 μm or less.

[0023] The difference between the maximum value and the minimum value of the thickness of the tube is preferably 5% or less with respect to the maximum value of the thickness.

[0024] Furthermore, according to the present invention, there is provided a method for producing a tube, which is the method for producing the above-mentioned tube, wherein the above-mentioned tube is obtained by molding the above-mentioned fluororesin at a line speed of 15 m / min or more.

[0025] Effects of the Invention

[0026] According to the present invention, there can be provided a fluororesin having high adhesion to other materials and capable of obtaining a tube having a smooth inner surface and a uniform thickness even when the tube is manufactured by extrusion molding at a high line speed. DETAILED DESCRIPTION

[0027] Hereinafter, specific embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.

[0028] The fluororesin of the present invention has a reactive functional group and a loss modulus (G" at 270°C) 270 ) and loss modulus at 280℃ (G” 280 ) (G” 270 -G" 280 ) is above 2500Pa.

[0029] In the production method described in Patent Document 1, a multilayer laminate with interlayer adhesion can be obtained by using a relatively high die temperature. However, due to the exposure of the fluororesin to a relatively high die temperature or the different melt viscosities of the polymer materials constituting each layer, there is a tendency for the interlayer adhesion strength to decrease, the inner surface of the obtained tube to become rough, or the thickness of the tube to vary. These disadvantages may become prominent in particular when extruding at a high temperature and a high line speed.

[0030] Therefore, the inventors have conducted intensive research on means for solving the above-mentioned problems while maintaining high adhesion to other materials. As a result, it has been found that, by using a fluororesin with a loss modulus at a specific temperature appropriately adjusted as a material for extrusion molding, a tube having a smooth inner surface and a uniform thickness can be manufactured while maintaining high adhesion to other materials even when extrusion molding is performed at a high line speed. In addition, a method for manufacturing a fluororesin with a loss modulus at a specific temperature appropriately adjusted has been discovered. The fluororesin of the present invention has been completed based on these findings.

[0031] The difference (G" of the fluororesin of the present invention 270 -G" 280 ) is 2500Pa or more. From the perspective of obtaining a tube with a smoother inner surface and a more uniform thickness, it is preferably 3000Pa or more, more preferably 3500Pa or more, and further preferably 4000Pa or more. The upper limit is not particularly limited, and is preferably 50000Pa or less, more preferably 20000Pa or less, and further preferably 10000Pa or less.

[0032] Fluorine resin difference (G" 270 -G" 280 ) is the loss modulus (G”) at 270°C 270 ) minus the loss modulus at 280°C (G”) 280 ) value. Storage modulus (G' 270 ) and storage modulus (G' 280 ) was measured under the conditions of strain 0.1% and angular frequency 10 rad / s. Loss modulus (G”) 270 ) and loss modulus (G” 280 ) is measured continuously. While heating the fluororesin, the loss modulus (G”) is measured when the temperature of the fluororesin reaches 270°C.270 ), then heat the fluororesin and measure the loss modulus (G") when the temperature of the fluororesin reaches 280°C 280 ).

[0033] In order to obtain a tube with a smoother inner surface and a more uniform thickness, the loss modulus (G”) of the fluororesin at 270°C 270 ) is preferably 5000Pa or more, more preferably 7000Pa or more, further preferably 9000Pa or more, preferably 60000Pa or less, more preferably 30000Pa or less, further preferably 20000Pa or less.

[0034] The difference (G') of the fluororesin of the present invention 270 -G' 280 ) is above 1500Pa. From the perspective of obtaining a tube with a smoother inner surface and a more uniform thickness, it is preferably above 1700Pa, more preferably above 1800Pa, and further preferably above 1900Pa. The upper limit is not particularly limited, but is preferably below 30000Pa, more preferably below 10000Pa, and further preferably below 7000Pa.

[0035] Fluorine resin difference (G' 270 -G' 280 ) is the storage modulus (G') at 270℃ 270 ) minus the storage modulus at 280°C (G' 280 ) value. Storage modulus (G' 270 ) and storage modulus (G' 280 ) was measured under the conditions of strain 0.1% and angular frequency 10 rad / s. Storage modulus (G' 270 ) and storage modulus (G' 280 While heating the fluororesin, the storage modulus (G') was measured when the temperature of the fluororesin reached 270°C. 270 ), then the fluororesin is heated and the storage modulus (G') is measured when the temperature of the fluororesin reaches 280°C. 280 ).

[0036] In order to obtain a tube with a smoother inner surface and a more uniform thickness, the storage modulus (G') of the fluororesin at 270°C 270 ) is preferably 2000Pa or more, more preferably 3000Pa or more, further preferably 4000Pa or more, preferably 40000Pa or less, more preferably 20000Pa or less, further preferably 10000Pa or less.

[0037] The loss modulus (G") and storage modulus (G') of the fluororesin can be adjusted by optimizing the type of polymerization initiator, the timing of adding the polymerization initiator during polymerization, the polymerization time, etc. when the fluororesin is produced by polymerizing the monomers constituting the fluororesin in the presence of a polymerization initiator.

[0038] The fluororesin of the present invention has a reactive functional group. Since the fluororesin of the present invention has a reactive functional group, it can be extruded at a high line speed and can show high adhesion to other materials. Therefore, by using the fluororesin of the present invention, a laminate and a multilayer tube with excellent interlayer bonding strength can be manufactured with high productivity. The fluororesin more preferably has a reactive functional group at the main chain end and / or side chain of the polymer. As the reactive functional group, it is preferred to select at least one of the group consisting of a carbonyl group, a hydroxyl group, a heterocyclic group and an amino group.

[0039] In the present invention, "carbonyl" is a carbon divalent group consisting of a carbon-oxygen double bond, and is represented by a group represented by -C(=O)-. The reactive functional group containing the above-mentioned carbonyl group is not particularly limited, and examples thereof include carbonate groups, carboxylic acid halides (haloformyl groups), formyl groups, carboxyl groups, ester bonds (-C(=O)O-), anhydride bonds (-C(=O)OC(=O)-), isocyanate groups, amide groups, imide groups (-C(=O)-NH-C(=O)-), carbamate bonds (-NH-C(=O)O-), carbamoyl groups (NH2-C(=O)-), carbamoyloxy groups (NH2-C(=O)O-), urea groups (NH2-C(=O)-NH-), aminooxalyl groups (NH2-C(=O)-C(=O)-), and the like, which contain a carbonyl group as a part of the chemical structure.

[0040] In an amide group, an imide group, a urethane bond, a carbamoyl group, a carbamoyloxy group, a urea group, an aminooxalyl group, etc., a hydrogen atom bonded to the nitrogen atom thereof may be substituted with a hydrocarbon group such as an alkyl group.

[0041] As the reactive functional group, from the perspective of easy introduction, moderate heat resistance of the fluororesin and good adhesion at relatively low temperatures, an amide group, a carbamoyl group, a hydroxyl group, a carboxyl group, a carbonate group, a carboxylic acid halide group and an acid anhydride bond are preferred, and an amide group, a carbamoyl group, a hydroxyl group, a carbonate group, a carboxylic acid halide group and an acid anhydride bond are more preferred.

[0042] As the reactive functional group, at least one selected from the group consisting of a carbonate group and a carboxylic acid halide group is preferred. The carbonate group and the carboxylic acid halide group may be groups described in International Publication No. 99 / 45044.

[0043] The fluororesin may be composed of a polymer having a reactive functional group at either the main chain terminal or the side chain of the polymer, or may be composed of a polymer having a reactive functional group at both the main chain terminal and the side chain. In the case where the main chain terminal has a reactive functional group, it may be present at both ends of the main chain or only at one end. In the case where the above-mentioned reactive functional group also has an ether bond, the reactive functional group may be further present in the main chain.

[0044] Fluororesins composed of a polymer having a reactive functional group at a main chain terminal are preferred because they do not significantly reduce mechanical properties and chemical resistance, or because they are advantageous in terms of productivity and cost.

[0045] The number of the reactive functional groups may be appropriately selected depending on the type, shape, purpose of bonding, application, required bonding strength, bonding method with the adjacent layer, and the like.

[0046] As for the number of reactive functional groups, from the viewpoint of obtaining higher adhesion, per 10 6 The number of carbon atoms in the main chain is preferably 3 to 800, more preferably 15 or more, further preferably 30 or more, particularly preferably 50 or more, and preferably 400 or less, more preferably 300 or less. In addition, when the fluororesin of the present invention has at least one selected from the group consisting of carbonate groups and carboxylic acid halide groups, the total number of carbonate groups and carboxylic acid halide groups is 10 6 The number of main chain carbon atoms is preferably 3 to 800, more preferably 15 or more, further preferably 30 or more, particularly preferably 50 or more, and is preferably 400 or less, more preferably 300 or less.

[0047] The number of reactive functional groups is calculated as follows: a fluororesin is compression molded at a molding temperature 50°C higher than its melting point and a molding pressure of 5 MPa, and an infrared absorption spectrum analysis is performed on the resulting film having a thickness of 50 μm to 200 μm using an infrared spectrophotometer. The spectrum is compared with the infrared absorption spectrum of a known film to determine the type of characteristic absorption of the reactive functional group, and the value is calculated from each difference spectrum using the following formula.

[0048] The number of reactive functional groups (per 10 6 Main chain carbon atoms) = (l×K) / t

[0049] l: absorbance

[0050] K: Correction coefficient

[0051] t: Film thickness (mm)

[0052] Table 1 shows the correction coefficients of the terminal reactive functional groups to be targeted.

[0053] [Table 1]

[0054] Table 1

[0055] Terminal Group <![CDATA[Absorption frequency (cm -1 )]]> Correction factor -OC(=O)OR 1817 1426 -COF 1884 405 -COOH 1813,(1795-1792),1775 455 <![CDATA[-COOCH3]]> 1795 355 <![CDATA[-CONH2]]> 3438 408 <![CDATA[-CH2OH]]> 3648 2325

[0056] The correction factors in Table 1 are used to calculate the 6 The number of reactive functional groups per main chain carbon atoms is the value determined from the infrared absorption spectrum of the model compound.

[0057] The carboxylic acid halide group may be decomposed into a carboxylic acid by heating or the like during molding of the fluororesin or over time. Therefore, it is considered that the fluororesin generally contains a carboxylic acid group derived therefrom in addition to the carbonate and / or carboxylic acid halide groups.

[0058] Examples of methods for introducing reactive functional groups into the ends of the main chain and / or side chains include: a method of introducing the reactive functional groups by copolymerizing a monomer (β) containing the reactive functional groups; a method of using a compound having or producing reactive functional groups as a polymerization initiator; a method of using a compound having or producing reactive functional groups as a chain transfer agent; a method of introducing reactive functional groups into a fluorinated polymer by polymer reaction; a method of combining these methods; etc.

[0059] The reactive functional group-containing monomer (β) used for introducing the reactive functional group by copolymerization is not particularly limited as long as it is a monomer copolymerizable with the monomer providing the fluororesin and has the above-mentioned reactive functional group.

[0060] The first monomer (β) includes aliphatic unsaturated carboxylic acids described in International Publication No. 2005 / 100420. The unsaturated carboxylic acid preferably has at least one polymerizable carbon-carbon unsaturated bond in one molecule and at least one carbonyloxy group (—C(═O)—O—) in one molecule.

[0061] The aliphatic unsaturated carboxylic acid may be an aliphatic unsaturated monocarboxylic acid or an aliphatic unsaturated polycarboxylic acid having two or more carboxyl groups. Examples of the aliphatic unsaturated monocarboxylic acid include unsaturated aliphatic monocarboxylic acids having 3 to 6 carbon atoms such as (meth)acrylic acid and crotonic acid.

[0062] Examples of the aliphatic unsaturated polycarboxylic acid include unsaturated aliphatic polycarboxylic acids having 3 to 6 carbon atoms, such as maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, aconitic acid, maleic anhydride, itaconic anhydride, and citraconic anhydride.

[0063] As the second monomer (β), there can be mentioned the following:

[0064] CX 7 2=CY 1 -(Rf 4 ) n -Z 2

[0065] (Where Z 2 is the above-mentioned reactive functional group; X 7 and Y 1 are the same or different, and are hydrogen atoms or fluorine atoms; Rf 4 An unsaturated compound represented by an alkylene group having 1 to 40 carbon atoms, a fluorinated oxyalkylene group having 1 to 40 carbon atoms, a fluorinated alkylene group having 2 to 40 carbon atoms having an ether bond, or a fluorinated oxyalkylene group having 2 to 40 carbon atoms having an ether bond; n is 0 or 1).

[0066] The content of the monomer (β) unit containing a reactive functional group introduced by copolymerization is preferably 0.05 mol% or more, more preferably 0.1 mol% or more. If it is too much, gelation or sulfurization reaction is likely to occur during heating and melting, so the upper limit of the content of the monomer (β) unit is preferably 5 mol%, more preferably 3 mol%.

[0067] In order to obtain a fluororesin having a carboxylic acid halide group, various methods can be used, for example, the fluororesin having a carbonate group can be heated to thermally decompose (decarboxylate) the fluororesin. The heating temperature varies depending on the type of carbonate group and the type of fluororesin, and the polymer itself is preferably heated at a temperature of 270°C or more, preferably 280°C or more, and particularly preferably 300°C or more. The upper limit of the heating temperature is preferably below the thermal decomposition temperature of the portion other than the carbonate group of the fluororesin.

[0068] The fluororesin may have a heterocyclic group or an amino group at the main chain terminal or the side chain terminal of the polymer.

[0069] The heterocyclic group refers to a group having a heteroatom (e.g., a nitrogen atom, a sulfur atom, or an oxygen atom) in the ring at the heterocyclic site, and may be a saturated ring or an unsaturated ring, a monocyclic ring, or a condensed ring. Among the heterocyclic groups, oxazolyl is preferred.

[0070] Amino group refers to a monovalent functional group obtained by removing hydrogen from ammonia, primary amine or secondary amine. Specifically, for example, it is a formula:

[0071] -NR 1 R 2

[0072] (Where R 1 and R 2The amino group may be the same or different and is a group represented by a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. Specific examples of the amino group include -NH2, -NH(CH3), -N(CH3)2, -NH(CH2CH3), -N(C2H5)2, and -NH(C6H5).

[0073] The melting point of the fluororesin is preferably 150°C or higher, more preferably 170°C or higher, further preferably 180°C or higher, particularly preferably 190°C or higher, and is preferably lower than 324°C, more preferably 320°C or lower, further preferably 300°C or lower, particularly preferably 280°C or lower, and most preferably 260°C or lower.

[0074] The melt flow rate (MFR) of the fluororesin at any temperature (e.g., 265°C or 297°C) in the general molding temperature range of 230°C to 350°C is preferably 0.5 g / 10 minutes or more, more preferably 1.0 g / 10 minutes or more, further preferably 1.5 g / 10 minutes or more, particularly preferably 2.0 g / 10 minutes or more, and most preferably 2.5 g / 10 minutes or more, and preferably 100 g / 10 minutes or less, more preferably 50 g / 10 minutes or less, further preferably 40 g / 10 minutes or less, and particularly preferably 35 g / 10 minutes or less. The melt flow rate can be determined, for example, by measuring the mass (g) of the fluororesin flowing out of a nozzle having an inner diameter of 2 mm and a length of 8 mm at any temperature (e.g., 265°C or 297°C) and any load (e.g., 2.16 kg or 5 kg) per unit time (10 minutes) using a melt flow indexer.

[0075] The fluororesin of the present invention is a partially crystalline fluorine-containing polymer, not a fluororubber, but a fluoroplastic. The fluororesin has a melting point and is thermoplastic. The fluororesin may be melt-processable or non-melt-processable. Since a tube can be produced with higher productivity in melt extrusion molding, a melt-processable fluororesin is preferred.

[0076] In the present invention, melt processability means that the polymer can be melted and processed using existing processing equipment such as an extruder and an injection molding machine. Therefore, the melt flow rate of the melt-processable fluororesin is usually 0.01 g / 10 min to 500 g / 10 min.

[0077] Examples of melt-processable fluororesins include tetrafluoroethylene (TFE) / perfluoro(alkyl vinyl ether) (PAVE) copolymers, tetrafluoroethylene (TFE) / hexafluoropropylene (HFP) copolymers, TFE / ethylene copolymers [ETFE], TFE / ethylene / HFP copolymers, chlorotrifluoroethylene (CTFE) / ethylene copolymers [ECTFE], polyvinylidene fluoride [PVdF], polychlorotrifluoroethylene [PCTFE], CTFE / TFE copolymers, TFE / vinylidene fluoride (VdF) copolymers [VT], polyvinyl fluoride [PVF], TFE / VdF / CTFE copolymers [VTC], and TFE / HFP / VdF copolymers.

[0078] Examples of PAVE include perfluoro(methyl vinyl ether) (PMVE), perfluoro(ethyl vinyl ether) (PEVE), and perfluoro(propyl vinyl ether) (PPVE). Among them, PPVE is preferred. One or more of these may be used.

[0079] The fluororesin may have a polymerization unit based on other monomers in an amount that does not impair the essential properties of each fluororesin. As the other monomers, for example, they may be appropriately selected from TFE, HFP, ethylene, propylene, perfluoro(alkyl vinyl ether), perfluoroalkylethylene, hydrofluoroolefin, fluoroalkylethylene, perfluoro(alkyl allyl ether), etc.

[0080] The fluororesin is preferably at least one selected from the group consisting of TFE / perfluoro(alkyl vinyl ether) (PAVE) copolymers, tetrafluoroethylene (TFE) / hexafluoropropylene (HFP) copolymers, TFE / ethylene copolymers [ETFE], TFE / ethylene / HFP copolymers, chlorotrifluoroethylene (CTFE) / ethylene copolymers [ECTFE], polychlorotrifluoroethylene [PCTFE], and CTFE / TFE copolymers; more preferably at least one selected from the group consisting of TFE / ethylene copolymers [ETFE], TFE / ethylene / HFP copolymers, chlorotrifluoroethylene (CTFE) / ethylene copolymers [ECTFE], polychlorotrifluoroethylene [PCTFE], and CTFE / TFE copolymers; further preferably at least one selected from the group consisting of TFE / ethylene copolymers [ETFE], TFE / ethylene / HFP copolymers, and CTFE / TFE copolymers; particularly preferably at least one selected from the group consisting of TFE / ethylene copolymers [ETFE] and TFE / ethylene / HFP copolymers; and most preferably TFE / ethylene / HFP copolymers.

[0081] In the present invention, the content of each monomer unit of the fluororesin can be calculated by appropriately combining NMR, FT-IR, elemental analysis, and fluorescent X-ray analysis according to the type of monomer.

[0082] In the TFE / HFP copolymer, the mass ratio of TFE / HFP is preferably 80 to 97 / 3 to 20, more preferably 84 to 92 / 8 to 16.

[0083] The TFE / HFP copolymer may be a binary copolymer composed of TFE and HFP, or may be a ternary copolymer further including a comonomer copolymerizable with TFE and HFP (eg, a TFE / HFP / PAVE copolymer).

[0084] The TFE / HFP copolymer is also preferably a TFE / HFP / PAVE copolymer comprising PAVE-based polymerized units.

[0085] In the TFE / HFP / PAVE copolymer, the mass ratio of TFE / HFP / PAVE is preferably 70 to 97 / 3 to 20 / 0.1 to 10, and more preferably 81 to 92 / 5 to 16 / 0.3 to 5.

[0086] In the TFE / PAVE copolymer, the mass ratio of TFE / PAVE is preferably 90 to 99 / 1 to 10, more preferably 92 to 97 / 3 to 8.

[0087] ETFE is a copolymer containing ethylene units and TFE units. By introducing ethylene units and TFE units into the copolymer, the difference (G" can be easily increased. 270 -G" 280 ), a tube with a smoother inner surface can be obtained, and it is also easy to stack with other materials to make a laminate. As ETFE, a copolymer in which the molar ratio of TFE unit to ethylene unit (TFE unit / ethylene unit) is preferably 20 / 80 or more and 90 / 10 or less. A more preferred molar ratio is 37 / 63 or more and 85 / 15 or less, and a further preferred molar ratio is 38 / 62 or more and 80 / 20 or less. The above-mentioned ETFE can also be a copolymer composed of TFE, ethylene, and a monomer that can be copolymerized with TFE and ethylene. As a monomer that can be copolymerized, the following formula can be cited.

[0088] CH2=CX 5 R 3 CF2=CFRf 3 CF2=CFORf 3 、CH2=C(Rf 3 )2

[0089] (Where X 5 Indicates H or F, Rf 3 represents a fluoroalkyl group containing or not containing an ether bond), wherein preferably selected from CF2=CFRf 3 CF2=CFORf 3 and CH2=CX5 R 3 At least one of the group consisting of fluorine-containing vinyl monomers represented by 4 (Where Rf 4 represents a perfluoroalkyl group having 1 to 5 carbon atoms) and Rf 3 CH2=CX is a fluoroalkyl group having 1 to 8 carbon atoms 5 R 3 At least one of the group consisting of the fluorine-containing vinyl monomers represented, more preferably HFP. In addition, as a monomer copolymerizable with TFE and ethylene, it can be an aliphatic unsaturated carboxylic acid such as itaconic acid and itaconic anhydride. In ETFE, the monomer unit copolymerizable with TFE and ethylene is preferably 0.1 mol% to 10 mol%, more preferably 0.1 mol% to 5 mol%, and particularly preferably 0.2 mol% to 4 mol%.

[0090] The TFE / ethylene copolymer is also preferably a TFE / ethylene / HFP copolymer containing polymerized units based on HFP (HFP units). In the TFE / ethylene / HFP copolymer, the molar ratio of TFE / ethylene / HFP is preferably 40 to 65 / 30 to 60 / 0.5 to 20, more preferably 40 to 65 / 30 to 60 / 0.5 to 10.

[0091] The melting point of ETFE is preferably 150°C or higher, more preferably 170°C or higher, further preferably 180°C or higher, particularly preferably 190°C or higher, preferably lower than 324°C, more preferably 320°C or lower, further preferably 300°C or lower, particularly preferably 270°C or lower, and most preferably 260°C or lower.

[0092] The MFR (297°C) of ETFE is preferably 0.5 g / 10 minutes or more, more preferably 1.0 g / 10 minutes or more, further preferably 1.5 g / 10 minutes or more, particularly preferably 2.0 g / 10 minutes or more, and most preferably 2.5 g / 10 minutes or more, and is preferably 100 g / 10 minutes or less, more preferably 50 g / 10 minutes or less, further preferably 40 g / 10 minutes or less, and particularly preferably 35 g / 10 minutes or less. The MFR of ETFE is measured at a temperature of 297°C and a load of 5 kg.

[0093] The melting point of the TFE / ethylene / HFP copolymer is preferably 150°C or higher, more preferably 170°C or higher, further preferably 180°C or higher, particularly preferably 190°C or higher, and is preferably lower than 324°C, more preferably 250°C or lower, further preferably 230°C or lower, particularly preferably 220°C or lower, and most preferably 210°C or lower.

[0094] The MFR (265°C) of the TFE / ethylene / HFP copolymer is preferably 0.5 g / 10 minutes or more, more preferably 1.0 g / 10 minutes or more, further preferably 1.5 g / 10 minutes or more, particularly preferably 2.0 g / 10 minutes or more, and most preferably 2.5 g / 10 minutes or more, preferably 100 g / 10 minutes or less, more preferably 50 g / 10 minutes or less, further preferably 40 g / 10 minutes or less, and particularly preferably 35 g / 10 minutes or less. The MFR of ETFE is measured at a temperature of 265°C and a load of 5 kg.

[0095] As ETFE, it is also preferable to use an ethylene / tetrafluoroethylene copolymer described in Japanese Patent Application Laid-Open No. 2019-90013.

[0096] Ethylene / CTFE copolymer (ECTFE) is a copolymer comprising ethylene units and CTFE units, preferably 46 mol% to 52 mol% of ethylene units and 54 mol% to 48 mol% of CTFE units relative to the total of ethylene units and CTFE units. ECTFE may be a binary copolymer consisting of only ethylene units and CTFE units, and may further contain a polymerization unit based on a monomer copolymerizable with ethylene and CTFE (e.g., a fluoroalkyl vinyl ether (PAVE) derivative).

[0097] The content of the polymerized units based on the monomer copolymerizable with ethylene and CTFE is preferably 0.01 mol% to 5 mol% based on the total of the ethylene units, CTFE units and the polymerized units based on the above copolymerizable monomers.

[0098] The MFR (230° C.) of ECTFE is preferably 0.5 g / 10 min to 100 g / 10 min. The MFR of ECTFE is measured under the conditions of a temperature of 230° C. and a load of 2.16 kg.

[0099] The CTFE / TFE copolymer contains CTFE units and TFE units. The CTFE / TFE copolymer particularly preferably contains CTFE units, TFE units, and monomer (α) units derived from a monomer (α) copolymerizable with these units.

[0100] The monomer (α) is not particularly limited as long as it is a monomer copolymerizable with CTFE and TFE, and examples thereof include ethylene (Et), VdF, CF2=CF-ORf 1 (Where Rf 1 is a perfluoroalkyl group having 1 to 8 carbon atoms) [PAVE], CX 3 X 4 =CX 5 (CF2)n X 6 (Where X 3 , X 4 and X 5 are the same or different and are hydrogen or fluorine atoms; X 6 is a hydrogen atom, a fluorine atom or a chlorine atom; n is an integer from 1 to 10), a vinyl monomer, CF2=CF-OCH2-Rf 2 (Where Rf 2 The alkyl perfluorovinyl ether derivatives are preferably at least one selected from the group consisting of PAVE, the above-mentioned vinyl monomers and alkyl perfluorovinyl ether derivatives, and more preferably at least one selected from the group consisting of PAVE and HFP.

[0101] As PAVE, CF2=CF-ORf is preferred 3 (Where Rf 3 The perfluoro(alkyl vinyl ether) represented by a perfluoroalkyl group having 1 to 5 carbon atoms includes, for example, perfluoro(methyl vinyl ether) [PMVE], perfluoro(ethyl vinyl ether) [PEVE], perfluoro(propyl vinyl ether) [PPVE], perfluoro(butyl vinyl ether) and the like. Among them, at least one selected from the group consisting of PMVE, PEVE and PPVE is more preferred, and PPVE is further preferred.

[0102] As the alkyl perfluorovinyl ether derivative, Rf 2 It is a perfluoroalkyl group having 1 to 3 carbon atoms, and more preferably CF2=CF-OCH2-CF2CF3.

[0103] The ratio of CTFE units to TFE units in the CTFE / TFE copolymer is preferably 15 mol% to 90 mol% for CTFE units and 85 mol% to 10 mol% for TFE units, more preferably 15 mol% to 50 mol% for CTFE units and 85 mol% to 50 mol% for TFE units, and even more preferably 15 mol% to 25 mol% for CTFE units and 85 mol% to 75 mol% for TFE units.

[0104] The CTFE / TFE copolymer preferably contains 90 mol% to 99.9 mol% of the total of the CTFE unit and the TFE unit, and 0.1 mol% to 10 mol% of the monomer (α) unit. If the monomer (α) unit is less than 0.1 mol%, the moldability, environmental stress cracking resistance, and fuel cracking resistance are likely to deteriorate, and if it exceeds 10 mol%, the fuel barrier property, heat resistance, and mechanical properties tend to be poor.

[0105] As the CTFE / TFE copolymer, a CTFE / TFE / PAVE copolymer is particularly preferred.

[0106] In the CTFE / TFE / PAVE copolymer, the above-mentioned PAVE includes perfluoro(methyl vinyl ether) [PMVE], perfluoro(ethyl vinyl ether) [PEVE], perfluoro(propyl vinyl ether) [PPVE], perfluoro(butyl vinyl ether), etc., among which at least one selected from the group consisting of PMVE, PEVE and PPVE is preferred, and PPVE is more preferred.

[0107] In the CTFE / TFE / PAVE copolymer, the PAVE unit preferably accounts for 0.5 mol% or more and preferably 5 mol% or less of all monomer units.

[0108] The melting point of the CTFE / TFE copolymer is preferably 120°C or higher, more preferably 140°C or higher, further preferably 150°C or higher, particularly preferably 160°C or higher, and most preferably 190°C or higher, and is preferably lower than 324°C, more preferably 320°C or lower, and further preferably 270°C or lower.

[0109] The MFR (297° C.) of the CTFE / TFE copolymer is preferably 0.5 g / 10 min or more, more preferably 2.0 g / 10 min or more, further preferably 3.0 g / 10 min or more, particularly preferably 4.0 g / 10 min or more, and most preferably 5.0 g / 10 min or more, and is preferably 100 g / 10 min or less, more preferably 50 g / 10 min or less, further preferably 40 g / 10 min or less, and particularly preferably 35 g / 10 min or less. The MFR of the CTFE / TFE copolymer is measured at a temperature of 297° C. and a load of 5 kg.

[0110] Fluororesin can be produced by polymerizing fluorine-containing monomers constituting fluororesin by polymerization methods such as suspension polymerization, solution polymerization, emulsion polymerization, and bulk polymerization. As the polymerization method, emulsion polymerization or suspension polymerization is preferred, and suspension polymerization is more preferred, from the perspective of easy introduction of reactive functional groups and easy adjustment of loss modulus and storage modulus. In the polymerization, various conditions such as temperature and pressure, polymerization initiator or other additives can be appropriately set according to the composition and amount of the fluororesin.

[0111] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical polymerization initiator can be used, and an oil-soluble radical polymerization initiator is preferred.

[0112] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, and the following may be cited as representative examples:

[0113] Dialkyl peroxydicarbonates such as di-n-propyl peroxydicarbonate, di-isopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate and di-2-ethoxyethyl peroxydicarbonate;

[0114] Peroxyesters such as tert-butyl peroxyisobutyrate and tert-butyl peroxypivalate;

[0115] Dialkyl peroxides such as di-tert-butyl peroxide;

[0116] Di[fluoro(or chlorofluoro)acyl]peroxides; etc.

[0117] Examples of the di[fluoro(or fluorochloro)acyl]peroxides include diacyl peroxides represented by [(RfCOO)-]2 (Rf is a perfluoroalkyl group, an ω-hydroperfluoroalkyl group or a fluorochloroalkyl group).

[0118] Examples of the di[fluoro(or chlorofluoro)acyl]peroxides include di(ω-hydro-dodecafluorohexanoyl)peroxide, di(ω-hydro-tetrafluoroheptanoyl)peroxide, di(ω-hydro-hexafluorononanoyl)peroxide, di(perfluoropropionyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluorovaleranoyl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, di(ω-chloro-hexafluorobutyryl ... (ω-chloro-decafluorohexanoyl) peroxide, bis(ω-chloro-tetrafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-perfluorobutyryl-peroxide, bis(dichloropentafluorobutyryl) peroxide, bis(trichlorooctafluorohexanoyl) peroxide, bis(tetrachloroundecanoyl) peroxide, bis(pentachlorotetrafluorodecanoyl) peroxide, bis(undecachlorotriacontafluorodocosanoyl) peroxide, and the like.

[0119] As the water-soluble free radical polymerization initiator, it can be a known water-soluble peroxide, for example, ammonium salts, potassium salts, sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, percarbonic acid, etc., organic peroxides such as disuccinic acid peroxide and diglutaric acid peroxide, tert-butyl peroxymaleate, tert-butyl hydroperoxide, etc. It is also possible to use a reducing agent such as sulfites in combination with the peroxide, and the amount used can be 0.1 to 20 times relative to the peroxide.

[0120] During the polymerization, a surfactant, a chain transfer agent, and a solvent may be used, and any conventionally known surfactants, chain transfer agents, and solvents may be used.

[0121] As the surfactant, known surfactants can be used, for example, nonionic surfactants, anionic surfactants, cationic surfactants, etc. can be used. Among them, fluorine-containing anionic surfactants are preferred, and more preferably, fluorine-containing anionic surfactants containing or not containing ether-bonded oxygen (that is, oxygen atoms can be inserted between carbon atoms) and straight-chain or branched fluorine-containing anionic surfactants with 4 to 20 carbon atoms are more preferred. The amount of surfactant added (relative to polymerization water) is preferably 50 ppm to 5000 ppm.

[0122] Examples of chain transfer agents include hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetates such as ethyl acetate and butyl acetate; alcohols such as methanol and ethanol; mercaptans such as methyl mercaptan; halogenated hydrocarbons such as carbon tetrachloride, chloroform, dichloromethane, and chloromethane, etc. The amount of chain transfer agent added can be changed depending on the chain transfer constant of the compound used, but is usually used in the range of 0.01% to 20% by mass relative to the polymerization solvent.

[0123] Examples of the solvent include water and a mixed solvent of water and alcohol.

[0124] In suspension polymerization, in addition to water, fluorine-based solvents can also be used. Examples of fluorine-based solvents include hydrochlorofluoroalkanes such as CH3CClF2, CH3CCl2F, CF3CF2CCl2H, CF2ClCF2CFHCl, etc.; chlorofluoroalkanes such as CF2ClCFClCF2CF3, CF3CFClCFClCF3, etc.; hydrofluoroalkanes such as CF3CFHCFHCF2CF2CF3, CF2HCF2CF2CF2CF2H, CF3CF2CF2CF2CF2CF2CF2H, etc.; CH3OC2F5, CH 3OC3F7CF3CF2CH2OCHF2, CF3CHFCF2OCH3, CHF2CF2OCH2F, (CF3)2CHCF2OCH3, CF3CF2CH2OCH2CHF2, CF3CHFCF2OCH2CF3 and other hydrofluoroethers; perfluorocyclobutane, CF3CF2CF2CF3, CF3CF2CF2CF2CF3, CF3CF2CF2CF2CF2CF3 and other perfluoroalkanes, among which perfluoroalkanes are preferred. From the perspective of suspension and economy, the amount of fluorine-based solvent used is preferably 10% to 100% by mass relative to the aqueous medium.

[0125] The polymerization temperature is not particularly limited and may be 0 to 100° C. The polymerization pressure may be appropriately determined depending on the type and amount of the solvent used and other polymerization conditions such as vapor pressure and polymerization temperature, and may generally be 0 to 9.8 MPaG.

[0126] The fluororesin of the present invention may be in any form, such as an aqueous dispersion, powder, or pellets.

[0127] The fluororesin of the present invention (or the composition containing the fluororesin of the present invention) may be added with various additives such as conductive materials, reinforcing agents, fillers, ultraviolet absorbers, pigments, etc. within the range that does not impair the purpose of the present invention. By using such additives, the properties of the fluororesin such as conductivity, surface hardness, wear resistance, charging properties, and weather resistance can be improved.

[0128] The fluororesin of the present invention (or the composition containing the fluororesin of the present invention) contains substantially no stabilizer such as a heat stabilizer, specifically, cuprous oxide (copper (I) oxide), cupric oxide (copper (II) oxide), cuprous iodide, or cupric iodide. "Substantially containing" means that cuprous oxide (copper (I) oxide), cupric oxide (copper (II) oxide), cuprous iodide, or cupric iodide is not actively added.

[0129] The laminate of the present invention comprises a fluororesin layer containing the above-mentioned fluororesin and a non-fluororesin layer containing a non-fluororesin.

[0130] The fluororesin layer is a layer containing the above-mentioned fluororesin. Since the laminate of the present invention has the fluororesin layer, the layers are firmly bonded together and have excellent oil resistance, fuel barrier properties, chemical resistance, low reagent permeability, heat resistance, weather resistance, and contamination resistance. In addition, the above-mentioned fluororesin has a loss modulus (G”) of 270°C. 270 ) and loss modulus at 280℃ (G” 280 ) (G” 270 -G" 280 ) is very large, so when the fluororesin layer is located at the outermost layer of the laminate, the surface smoothness of the laminate is excellent.

[0131] In addition to the above-mentioned fluororesin, the fluororesin layer may further contain a conductive filler. By containing a conductive filler, it is possible to prevent the accumulation of static electricity generated by friction between the fuel or reagent and the laminate of the present invention, and it is possible to prevent fire or explosion that may be caused by static electricity discharge, or cracks or openings in the laminate of the present invention and fuel leakage caused thereby.

[0132] The conductive filler is not particularly limited, and examples thereof include conductive single powders or conductive single fibers of metals, carbon, etc.; powders of conductive compounds such as zinc oxide; and powders subjected to surface conductivity treatment.

[0133] The above-mentioned conductive single powder or conductive single fiber is not particularly limited, and examples thereof include: metal powders such as copper and nickel; metal fibers such as iron and stainless steel; carbon black, carbon fiber, carbon fibrils described in Japanese Patent Gazette No. 3-174018, carbon nanotubes, carbon nanohorns, etc.

[0134] The surface conductive powder is a powder obtained by applying a conductive treatment to the surface of a non-conductive powder such as glass beads or titanium oxide. The method of the conductive treatment is not particularly limited, and examples thereof include metal sputtering and electroless plating. Among the conductive fillers, carbon black is advantageous from the perspective of economic efficiency and is therefore preferably used.

[0135] The amount of the conductive filler is appropriately determined based on the type of perfluororesin, the conductive properties required for the laminate, molding conditions, etc., and is preferably 1 to 30 parts by mass relative to 100 parts by mass of the perfluororesin. The more preferred lower limit is 5 parts by mass, and the more preferred upper limit is 20 parts by mass.

[0136] In addition to the conductive filler, various additives such as reinforcing agents, fillers, ultraviolet absorbers, pigments, etc. may be added to the fluororesin layer within the scope that does not impair the purpose of the present invention. By using such additives, the properties of the fluororesin layer such as surface hardness, wear resistance, charging, and weather resistance can be improved.

[0137] The non-fluorine resin layer is a layer containing a non-fluorine resin. Since the laminate of the present invention includes the non-fluorine resin layer, in addition to the excellent effects obtained by including the fluorine resin layer, the excellent effects obtained by including the non-fluorine resin layer are also obtained.

[0138] Examples of the non-fluorine-free resin include polyamide resins, polyolefin resins, vinyl chloride resins, polyurethane resins, polyester resins, polyaramid resins, polyimide resins, polyamide-imide resins, polyphenylene ether resins, polyacetal resins, polycarbonate resins, acrylic resins, styrene resins, acrylonitrile / butadiene / styrene resins [ABS], cellulose resins, polyetheretherketone resins [PEEK], polysulfone resins, polyethersulfone resins [PES], polyetherimide resins, and resins having excellent mechanical strength and mainly functioning to maintain pressure resistance and molded body shape (hereinafter referred to as structural component resins), and ethylene / vinyl alcohol copolymer resins, polyphenylene sulfide resins, polybutylene naphthalate resins, polybutylene terephthalate resins, polyphthalamide [PPA], and other resins having high resistance to the permeation of fuels or gases (hereinafter referred to as permeation-resistant resins).

[0139] The non-fluorine-free resin is preferably at least one selected from the group consisting of polyamide resins, ethylene / vinyl alcohol copolymer resins and polyolefin resins, more preferably at least one selected from the group consisting of polyamide resins and ethylene / vinyl alcohol copolymer resins, and still more preferably polyamide resins.

[0140] The laminate of the present invention has excellent mechanical strength when the non-fluororesin layer contains the above-mentioned structural member resin, and has excellent resistance to fuel permeation when the non-fluororesin layer contains the above-mentioned permeation resistance resin.

[0141] The polyamide resin is composed of a polymer having an amide bond [—NH—C(═O)—] as a repeating unit in the molecule.

[0142] The polyamide resin may be a so-called nylon resin composed of a polymer having an amide bond and an aliphatic structure or an alicyclic structure bonded thereto in a molecule, or a so-called aromatic polyamide resin composed of a polymer having an amide bond and an aromatic structure bonded thereto in a molecule.

[0143] The polyamide resin (nylon resin) is not particularly limited and includes, for example, materials composed of polymers such as polyamide 6, polyamide 66, polyamide 11, polyamide 12, polyamide 610, polyamide 1010, polyamide 612, polyamide 6 / 66, polyamide 66 / 12, polyamide 46, meta-xylylenediamine / adipic acid copolymer, polyamide 62, polyamide 92, polyamide 122, polyamide 142, and aromatic polyamides such as polyamide 6T and polyamide 9T, and two or more of them may be used in combination.

[0144] The aramid resin is not particularly limited, and examples thereof include poly(p-phenylene terephthalamide) and poly(meta-phenylene isophthalamide).

[0145] Polyamide resin can also be a resin composed of a polymer block copolymerized or grafted on a part of the molecule without an amide bond as a repeating unit. As such a polyamide resin, for example, a resin composed of polyamide elastomers such as polyamide 6 / polyester copolymer, polyamide 6 / polyether copolymer, polyamide 12 / polyester copolymer, polyamide 12 / polyether copolymer, etc. can be cited. These polyamide elastomers are obtained by copolymerizing polyamide oligomers and polyester oligomers by ester bond blocks, or by copolymerizing polyamide oligomers and polyether oligomers by ether bond blocks. As the above-mentioned polyester oligomers, for example, polycaprolactone, polyethylene adipate, etc. can be cited, and as the above-mentioned polyether oligomers, for example, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, etc. can be cited. As the above-mentioned polyamide elastomers, polyamide 6 / polytetramethylene glycol copolymers and polyamide 12 / polytetramethylene glycol copolymers are preferred.

[0146] As a polyamide resin, sufficient mechanical strength can be obtained even if the layer composed of the polyamide resin is thin. Therefore, polyamide 6, polyamide 66, polyamide 11, polyamide 12, polyamide 610, polyamide 1010, polyamide 612, polyamide 62, polyamide 6 / 66, polyamide 66 / 12, polyamide 6 / polyester copolymer, polyamide 6 / polyether copolymer, polyamide 12 / polyester copolymer, polyamide 12 / polyether copolymer, etc. are preferred, and two or more of them can also be used in combination.

[0147] The amine value of the polyamide resin is preferably 10 to 80 (equivalent / 10 6 g). If the amine value is within the above range, even when coextrusion is performed at a relatively low temperature, the interlayer adhesion can be excellent. 6 If the amount exceeds 80 (equivalent weight / 10 6 g), the mechanical strength of the laminate is insufficient, and it is easy to color during storage, and the handling properties may be deteriorated. A more preferred lower limit is 15 (equivalent / 10 6 g), and a further preferred lower limit is 23 (equivalent / 10 6 g), and a more preferred upper limit is 60 (equivalent / 10 6 g), and a further preferred upper limit is 50 (equivalent / 10 6 g).

[0148] In the present invention, the amine value is a value obtained by dissolving 1 g of a polyamide resin in 50 ml of m-cresol by heating and titrating the solution with a 1 / 10 equivalent aqueous p-toluenesulfonic acid solution using thymol blue as an indicator, and unless otherwise specified, refers to the amine value of the polyamide resin before lamination. It is believed that a portion of the amino groups in the polyamide resin before lamination is consumed in bonding with the adjacent layers, but the number of amino groups is extremely small relative to the entire layer, so the amine value of the polyamide resin before lamination is substantially the same as the amine value in the laminate of the present invention.

[0149] The polyolefin resin is a resin having a monomer unit derived from a vinyl-containing monomer having no fluorine atom. The vinyl-containing monomer having no fluorine atom is not particularly limited, but is preferably a monomer having a polar functional group in applications requiring interlayer adhesion.

[0150] The polyolefin resin is not particularly limited. For example, in addition to polyolefins such as polyethylene, polypropylene, high-density polyolefins, and low-density polyolefins, there can also be mentioned modified polyolefins obtained by modifying the above polyolefins using maleic anhydride or the like, epoxy-modified polyolefins, amine-modified polyolefins, etc., among which high-density polyolefins are preferred.

[0151] The ethylene / vinyl alcohol copolymer resin is obtained by saponifying an ethylene / vinyl acetate copolymer obtained from ethylene and vinyl acetate. The blending ratio of the copolymerized ethylene and vinyl acetate is appropriately determined according to the ratio of the number of moles of vinyl acetate units specified by the following formula.

[0152] The ethylene / vinyl alcohol copolymer resin preferably has vinyl acetate units X mol% and saponification degree Y% satisfying X×Y / 100≥7. If X×Y / 100<7, the interlayer adhesion may be insufficient. More preferably, X×Y / 100≥10. The value of X×Y / 100 is an indicator of the content of hydroxyl groups in the ethylene / vinyl alcohol copolymer resin, and a large value of X×Y / 100 means that the content of hydroxyl groups in the ethylene / vinyl alcohol copolymer resin is high.

[0153] The hydroxyl group is a group that can participate in the adhesion between the EVOH layer and the laminated object material. If the hydroxyl content of the ethylene / vinyl alcohol copolymer resin is high, the interlayer adhesion in the laminate is improved. In the present invention, the above-mentioned "laminated object material" refers to a material that is in contact and laminated.

[0154] In the present invention, "X mol% of vinyl acetate units" refers to the ratio of the number of moles of vinyl acetate derived from the vinyl acetate units [Ni] to the total number of moles of ethylene and vinyl acetate added to the molecule of the ethylene / vinyl alcohol copolymer resin [N], and is expressed by the following formula:

[0155] Xi(%)=(Ni / N)×100

[0156] The molar content Xi is an average value. The vinyl acetate unit X mol% is a value obtained by measuring using an infrared absorption spectrum [IR].

[0157] In the present invention, the "vinyl acetate unit" is a part of the molecular structure of the ethylene / vinyl alcohol copolymer resin, and refers to a part derived from vinyl acetate. The vinyl acetate unit may be saponified to have a hydroxyl group, or may be unsaponified to have an acetoxy group.

[0158] The “saponification degree” is a percentage indicating the ratio of the number of saponified vinyl acetate units to the total number of saponified vinyl acetate units and the number of unsaponified vinyl acetate units. The saponification degree is a value obtained by measuring using infrared absorption spectroscopy [IR].

[0159] Examples of the ethylene / vinyl alcohol copolymer resin in which X and Y satisfy the above formula include commercially available products such as EVAL F101 (manufactured by KURARAY CO., LTD., vinyl acetate unit X=68.0 mol %; saponification degree Y=95%; X×Y / 100=64.6), Melthene H6051 (manufactured by Tosoh CO., LTD., vinyl acetate unit X=11.2 mol %; saponification degree Y=100%; X×Y / 100=11.2), and TECHNOLINK K200 (manufactured by Taoka Chemical Co., Ltd., vinyl acetate unit X=11.2 mol %; saponification degree Y=85%; X×Y / 100=9.52).

[0160] The MFR of the ethylene / vinyl alcohol copolymer resin at 200°C is preferably 0.5 g / 10 min to 100 g / 10 min. If the MFR is less than 0.5 g / 10 min or exceeds 100 g / 10 min, the difference between the melt viscosity of the ethylene / vinyl alcohol copolymer resin and the melt viscosity of the counterpart material tends to become larger, and the thickness of each layer may be uneven, which is not preferred. The preferred lower limit is 1 g / 10 min, and the preferred upper limit is 50 g / 10 min.

[0161] The melting point of the non-fluorine resin is preferably 50° C. to 400° C. The lower limit is more preferably 100° C., and further preferably 150° C. The upper limit is more preferably 300° C., and further preferably 250° C.

[0162] The melting point was determined as the temperature corresponding to the maximum value in the heat of fusion curve when the temperature was increased at a rate of 10° C. / min using a differential scanning calorimeter (DSC) apparatus (manufactured by SEIKO Corporation).

[0163] The non-fluorine resin layer may be added with various additives such as stabilizers such as heat stabilizers, reinforcing agents, fillers, ultraviolet absorbers, pigments, etc. within the scope that does not impair the purpose of the present invention. By using such additives, the properties of the non-fluorine resin such as thermal stability, surface hardness, wear resistance, charging, and weather resistance can be improved.

[0164] The laminate of the present invention preferably comprises a fluororesin layer and a polyamide resin layer containing a polyamide resin as a non-fluororesin layer. In the laminate of the present invention, since an excellent interlayer bonding strength can be obtained without providing an adhesive layer, etc., it is preferred that the fluororesin layer and the polyamide resin layer are directly bonded. As the laminate of the present invention, for example, a laminate having a fluororesin layer / polyamide resin layer as the innermost layer / outermost layer can be cited. The laminate having a fluororesin layer and a polyamide resin layer can have both the excellent properties of fluororesin such as oil resistance, fuel barrier property, chemical resistance, low reagent permeability, heat resistance, weather resistance, and pollution resistance and the properties of polyamide resin such as high strength, high toughness, light weight, excellent processability, and particularly softness.

[0165] When the polyamide resin has the above amine value, the fluororesin layer and the polyamide resin layer can be particularly firmly bonded to each other. The interlayer bonding strength between the fluororesin layer and the polyamide resin layer is preferably 30 N / cm or more.

[0166] The interlayer adhesive strength was determined by performing a 180° peel test at a speed of 25 mm / min using a Tensilon universal testing machine.

[0167] The laminate of the present invention preferably comprises a fluororesin layer and an EVOH layer containing an ethylene / vinyl alcohol copolymer (EVOH) resin. The laminate comprising a fluororesin layer and an EVOH layer can have both excellent properties of fluororesin such as oil resistance, fuel barrier properties, chemical resistance, low reagent permeability, heat resistance, weather resistance, and contamination resistance and excellent properties of EVOH such as fuel barrier properties and low reagent permeability.

[0168] In the laminate of the present invention, since excellent interlayer bonding strength can be obtained and excellent properties of three resins can be obtained, it is more preferable to have a polyamide resin layer in addition to the fluororesin layer and the EVOH layer. In the laminate of the present invention, since excellent interlayer bonding strength can be obtained without providing an adhesive layer, etc., it is preferable that the fluororesin layer is directly bonded to the polyamide resin layer, and the polyamide resin layer is directly bonded to the EVOH layer.

[0169] Examples of the laminate of the present invention include:

[0170] A laminate having a fluororesin layer / polyamide resin layer as the innermost layer / outermost layer;

[0171] As the innermost layer / intermediate layer / outermost layer, a laminate of a fluororesin layer / EVOH layer / polyamide resin layer, or a laminate of a fluororesin layer / polyamide resin layer / EVOH layer;

[0172] A laminate having a fluororesin layer / polyamide resin layer / EVOH layer / polyamide resin layer as the innermost layer / inner layer / middle layer / outermost layer;

[0173] As the innermost layer / inner layer / intermediate layer / outer layer / outermost layer, a laminate comprising a fluororesin layer / polyamide resin layer / EVOH layer / polyamide resin layer / polyamide resin layer, and a laminate comprising a fluororesin layer / polyamide resin layer / EVOH layer / polyamide resin layer / polyolefin resin layer;

[0174] As the innermost layer / inner layer 1 / inner layer 2 / intermediate layer / outer layer / outermost layer, there are laminates comprising a fluororesin layer / polyamide resin layer / polyamide resin layer / EVOH layer / polyamide resin layer / polyamide resin layer, laminates comprising a fluororesin layer / polyamide resin layer / EVOH layer / polyamide resin layer / polyamide resin layer / polyolefin resin layer, laminates comprising a fluororesin layer / polyamide resin layer / EVOH layer / polyamide resin layer / polyolefin resin layer / polyamide resin layer, laminates comprising a fluororesin layer / fluororesin layer / polyamide resin layer / EVOH layer / polyamide resin layer / polyolefin resin layer, fluororesin layer / polyamide resin layer / polyolefin resin layer / polyamide resin layer / polyamide resin layer, etc.

[0175] When the laminate of the present invention has more than two fluororesin layers, the type of fluororesin contained in each layer may be the same or different. When the laminate of the present invention has more than two polyamide resin layers, the type of polyamide resin contained in each layer may be the same or different. When the laminate of the present invention has more than two EVOH layers, the type of ethylene / vinyl alcohol copolymer contained in each layer may be the same or different. In the laminate of the present invention, the boundaries between the adjacent layers do not necessarily need to be clear, and the layer structure may also be one in which the molecular chains of the polymers constituting each layer intrude into each other from the surfaces in contact with each other and have a concentration gradient.

[0176] The laminate of the present invention may have other layers. The thickness, shape, etc. of each layer of the laminate of the present invention may be appropriately selected according to the purpose of use, form of use, etc.

[0177] The single-layer tube (hose) of the present invention contains the above-mentioned fluororesin. The multi-layer tube (hose) of the present invention is formed by the above-mentioned laminate. In any tube, it is preferred that the inner surface of the tube is formed by the above-mentioned fluororesin. The above-mentioned fluororesin has a loss modulus (G" at 270°C) of 1.5 % and ... 270 ) and loss modulus at 280℃ (G” 280 ) (G” 270 -G" 280 ) is very large, so the inner surface of the tube formed of the above-mentioned fluororesin can be made very smooth. The surface roughness Ra of the inner surface of the tube is, for example, 1.0 μm or less, preferably 0.5 μm or less, more preferably 0.2 μm or less, and can be 0.01 μm or more. The surface roughness can be measured in accordance with JIS B0601-1994.

[0178] The tube of the present invention comprises at least the fluororesin layer containing the fluororesin. The fluororesin has a loss modulus (G" at 270°C) of 270 ) and loss modulus at 280℃ (G” 280 ) (G” 270 -G"280 ) is very large, therefore, the tube of the present invention has a uniform thickness regardless of whether it is a single-layer tube or a multi-layer tube formed of a laminate. The difference between the maximum value and the minimum value of the tube thickness is, for example, 5% or less, preferably 3% or less, and more preferably 2% or less relative to the maximum value of the thickness.

[0179] The outer diameter of the tube is preferably 2 mm to 20 mm, more preferably 3 mm or more, further preferably 4 mm or more, most preferably 6 mm or more, more preferably 18 mm or less, further preferably 16 mm or less, most preferably 14 mm or less.

[0180] The inner diameter of the tube is preferably 1 mm to 15 mm, more preferably 2 mm or more, further preferably 3 mm or more, most preferably 4 mm or more, more preferably 13 mm or less, further preferably 11 mm or less, most preferably 10 mm or less.

[0181] The thickness of the tube (the difference between the outer diameter and the inner diameter) is preferably 0.5 mm to 8 mm, more preferably 0.6 mm to 6 mm, further preferably 0.6 mm to 4 mm, and most preferably 0.7 mm to 2 mm.

[0182] The thickness of the fluororesin layer in the laminate and tube is preferably 0.05 to 0.4 mm, more preferably 0.06 to 0.3 mm, and even more preferably 0.07 to 0.25 mm. When the laminate and tube have two or more fluororesin layers, the thickness of the fluororesin layer is the total thickness of each layer.

[0183] The thickness of the non-fluororesin layer in the laminate and the tube is preferably 0.05 to 4 mm, more preferably 0.1 to 3 mm, and even more preferably 0.5 to 2 mm. When the laminate and the tube have two or more non-fluororesin layers, the thickness of the non-fluororesin layer is the total thickness of each layer.

[0184] When the laminate and the tube have a two-layer structure of innermost layer / outermost layer, the thickness of the innermost layer is preferably 0.05 mm to 0.4 mm, more preferably 0.06 mm to 0.3 mm, and even more preferably 0.07 mm to 0.25 mm. The thickness of the outermost layer is preferably 0.05 mm to 4 mm, more preferably 0.1 mm to 3 mm, and even more preferably 0.5 mm to 2 mm.

[0185] When the laminate and the tube have a five-layer structure of innermost layer / inner layer / intermediate layer / outer layer / outermost layer, the thickness of the innermost layer is preferably 0.01 mm to 0.5 mm, more preferably 0.02 mm to 0.25 mm, and even more preferably 0.03 mm to 0.15 mm.

[0186] The thickness of the inner layer is preferably 0.01 mm to 1.0 mm, more preferably 0.03 mm to 0.5 mm, and even more preferably 0.05 mm to 0.3 mm.

[0187] The thickness of the intermediate layer is preferably 0.01 mm to 0.5 mm, more preferably 0.02 mm to 0.25 mm, and even more preferably 0.03 mm to 0.15 mm.

[0188] The thickness of the outer layer is preferably 0.01 mm to 1.0 mm, more preferably 0.03 mm to 0.5 mm, and even more preferably 0.05 mm to 0.3 mm.

[0189] The thickness of the outermost layer is preferably 0.01 mm to 1.0 mm, more preferably 0.03 mm to 0.7 mm, and even more preferably 0.05 mm to 0.5 mm.

[0190] The fluororesin of the present invention has excellent oil resistance, fuel barrier properties, chemical resistance, low reagent permeability, heat resistance, weather resistance, and pollution resistance, and can therefore be used in various fields such as semiconductors, automobiles, construction, electrical / electronics, chemical equipment, and medicine. In addition, the fluororesin of the present invention has high adhesion to other materials. By using the fluororesin of the present invention, even when a tube is manufactured by extrusion molding at a high line speed, a tube with a smooth inner surface and a uniform thickness can be obtained with strong adhesion between layers. The fluororesin of the present invention can be extruded not only at a high line speed, but also at a low line speed. Therefore, the fluororesin of the present invention can be particularly suitable for laminates, tubes, and the like.

[0191] By molding the fluororesin of the present invention, various molded products such as films, sheets, tubes (tubes), bottles, and cans can be obtained. The molded products containing the fluororesin of the present invention are excellent in oil resistance, fuel barrier properties, chemical resistance, low reagent permeability, heat resistance, weather resistance, and contamination resistance.

[0192] The laminate of the present invention can be formed into various shapes such as film, sheet, tube (hose), bottle, can, etc. The film, sheet, tube, and hose shapes may be corrugated, corrugated, or convoluted.

[0193] The tube (hose) may be in a corrugated shape, a serpentine shape, a convoluted shape, etc. When the tube (hose) has a corrugated shape, the corrugated folds are arranged in a plurality of annular regions, so that one side of the annular region can be compressed and the other side can be expanded outward in the region, so that it can be easily bent at any angle without stress fatigue or interlayer peeling.

[0194] The method for forming the corrugated region is not limited, and the corrugated region can be easily formed by first molding a straight tube and then performing molding or the like to form a predetermined corrugated shape.

[0195] There is no particular limitation on the molding method of the fluororesin, and examples thereof include heat compression molding, transfer molding, extrusion molding, injection molding, and calendaring molding. During molding, commonly used fluoropolymer molding machines, such as injection molding machines, blow molding machines, extrusion molding machines, and various coating devices can be used, and molded products and laminates in various shapes such as sheets and tubes can be manufactured. In addition, multi-layer molded products such as multi-layer tubes, multi-layer hoses, and multi-layer tanks can be manufactured by molding methods such as multi-layer extrusion molding, multi-layer blow molding, and multi-layer injection molding.

[0196] Examples of the method for producing the laminate of the present invention include:

[0197] (1) A method of forming a laminate of a multilayer structure in one stage by co-extrusion molding of polymers forming each layer to thermally fuse (melt-bond) the layers (co-extrusion molding);

[0198] (2) A method in which layers produced separately by an extruder are overlapped and bonded to each other by heat fusion;

[0199] (3) A method of forming a laminate by extruding a polymer forming a layer adjacent to the layer onto the surface of a previously produced layer using an extruder;

[0200] (4) A method of electrostatically coating the surface of a previously formed layer with a polymer that will form a layer adjacent to the layer, and then heating the entire resulting coated material or heating it from the coated side to heat and melt the coated polymer to form the layer; etc.

[0201] In the case where the laminate of the present invention is a tube or a hose, for example, as a method equivalent to the above (2), there can be cited (2a) a method in which each cylindrical layer is formed separately by an extruder, and a coating of a layer in contact with the layer is formed on the layer becoming the inner layer in the form of a heat shrink tube; as a method equivalent to the above (3), there can be cited (3a) a method in which a layer becoming the inner layer is first formed by an inner layer extruder, and a layer in contact with the layer is formed on its outer peripheral surface by an outer layer extruder; as a method equivalent to the above (4), there can be cited (4a) a method in which a polymer constituting the inner layer is electrostatically coated on the inner side of the layer in contact with the layer, and the resulting coated article is placed in a heating oven for heating as a whole, or a rod-shaped heating device is inserted into the inner side of the cylindrical coated article to heat it from the inside, thereby heating and melting the polymer constituting the inner layer for molding; and the like.

[0202] If the layers constituting the laminate and tube of the present invention can be coextruded, they are usually formed by the coextrusion molding described in (1). Examples of the coextrusion molding include conventionally known multi-layer coextrusion production methods such as the multi-manifold method and the feedblock method.

[0203] In the molding methods (2) and (3) above, after forming each layer, the contact surface of each layer with other layers may be subjected to surface treatment in order to improve interlayer adhesion. Examples of such surface treatment include etching treatment such as sodium etching treatment; corona treatment; and plasma treatment such as low-temperature plasma treatment.

[0204] The method for forming the laminate of the present invention may also be a method for forming a laminate by rotating two or more materials in multiple stages. In this case, the melting point of the outer layer material does not need to be higher than that of the inner layer material, and the melting point of the inner layer material may be higher than that of the outer layer material by 100°C or more. In this case, it is preferred that a heating portion is also provided inside.

[0205] The laminate and tube of the present invention have a loss modulus (G" at 270°C) 270 ) and loss modulus at 280℃ (G” 280 ) (G” 270 -G" 280 ) is a very large fluororesin, so it can be manufactured by extruding the fluororesin at a high line speed. As the line speed, it is preferably 15m / min or more, more preferably 20m / min or more, and can also be 100m / min or less. Even if the laminate of the present invention is obtained by molding at such a high line speed, the layers are firmly bonded and the surface is smooth. Even if the tube of the present invention is obtained by molding at such a high line speed, the inner surface is smooth. The laminate and tube of the present invention can also be manufactured by extruding the fluororesin at a low line speed. The line speed can be, for example, 8m / min to 100m / min.

[0206] The laminate and the tube of the present invention can be manufactured by molding fluororesin and other materials as required using an extrusion molding machine. The extrusion molding machine is not particularly limited, and an extrusion molding machine having a barrel, a die adapter, and a spiral multi-flow die or a right-angle die head die with a die head and a die head front end can be used.

[0207] An extrusion molding machine is usually composed of a feed hopper, a screw, a barrel, a die adapter (the connecting part between the screw and the die), and a die. An extrusion molding machine equipped with a screw can be a single-screw extruder or a twin-screw extruder. A vent hole can also be provided in the barrel, and the vent hole can be opened or decompressed to remove the volatile components generated by the fluororesin.

[0208] The barrel temperature is preferably 150°C to 350°C, more preferably 180°C to 330°C. The die temperature is preferably 230°C to 330°C, more preferably 250°C to 320°C. The front end temperature is preferably 230°C to 330°C, more preferably 250°C to 320°C. By setting the die temperature and the front end temperature within the above range, a laminate with a smoother surface or a tube with a smoother inner surface can be obtained. In particular, when a laminate or a multilayer tube is manufactured by co-extrusion molding of a polyamide resin or an ethylene / vinyl alcohol copolymer resin with a fluororesin (such as ETFE), it is preferably set to the above-mentioned die temperature and the front end temperature in order to obtain a laminate with a smoother surface or a tube with a smoother inner surface.

[0209] The fluororesin, laminate and tube of the present invention can be used in the following applications.

[0210] Films and sheets: food films, food sheets, chemical films, anti-adhesive films, chemical sheets, agricultural films, diaphragms of diaphragm pumps or various sealing gaskets, etc.;

[0211] Tubes and hoses: tubes or hoses for chemical reagents, tubes or hoses for paint (including those for printing machines), tubes or hoses for automobile fuel and other fuel tubes or hoses, tubes or hoses for solvents, automobile radiator hoses, air conditioning hoses, brake hoses, wire covering materials, tubes or hoses for beverages and foods, underground buried tubes or hoses for gas stations, tubes or hoses for submarine oil fields (including injection tubes and crude oil pipelines), etc.

[0212] Bottles, containers, and cans: automobile radiator tanks, gasoline tanks and other fuel tanks, solvent tanks, paint tanks, chemical reagent containers such as semiconductor chemical reagent containers, beverage and food cans, etc.;

[0213] Others: carburetor flange gaskets, fuel pump O-rings and other automotive seals, hydraulic equipment seals and other mechanical seals, gears, medical tubes (including catheters), cableway tubes, etc.

[0214] Although the embodiments have been described above, it will be understood that various changes in form and details may be made without departing from the spirit and scope of the claims.

[0215] Example

[0216] Next, although an embodiment of the present invention will be described with reference to examples, the present invention is not limited to the examples.

[0217] Each numerical value in the examples was measured by the following method.

[0218] <Polymer composition>

[0219] The fluororesin pellets obtained in the examples were used and a nuclear magnetic resonance apparatus AC300 (manufactured by Bruker-Biospin) for nuclear magnetic resonance. 19 The polymer composition was determined from the integrated value of each peak by F-NMR measurement. In addition, the polymer composition (the content of each monomer unit in the polymer) was determined by appropriately combining the results of elemental analysis according to the types of monomers.

[0220] <Melting point>

[0221] Using the pellets of the fluororesin obtained in Examples and a differential scanning calorimeter RDC220 (manufactured by Seiko Instruments), thermal measurement was performed at a heating rate of 10°C / min in accordance with ASTM D 4591, and the melting point of the fluororesin was determined from the peak of the obtained endothermic curve.

[0222] <Melt Flow Rate (MFR)>

[0223] Using the pellets of the fluororesin obtained in the examples and a melt flow indexer (manufactured by Yasuda Seiki Co., Ltd.), the mass (g / 10 minutes) of the fluororesin flowing out of a nozzle having an inner diameter of 2 mm and a length of 8 mm per 10 minutes at 265°C or 297°C and a load of 5 kg was determined as MFR in accordance with ASTM D 1238.

[0224] <Number of Carbonate Groups and Carboxylic Acid Fluoride Groups>

[0225] The pellets of the fluororesin obtained in the example were compression molded at room temperature to produce a film with a thickness of 50 μm to 200 μm. According to the infrared absorption spectrum analysis of the film, at 1817 cm -1 [ν (C=O) The absorption wavelength of ] shows the peak of the carbonyl group of carbonate group [-OC(=O)O-] at 1884 cm -1 [ν (C=O) ] appears at the absorption wavelength derived from the carbonyl group of the carboxylic acid fluoride group [-COF], so the ν (C=O) The absorbance of the peak was calculated by the following formula: 6 The number of carbon atoms in the main chain.

[0226] The number of carbonate groups or carboxylic acid fluoride groups (per 10 6 Main chain carbon atoms) = (l×K) / t

[0227] l: absorbance

[0228] K: Correction coefficient (-OC(=O)OR: 1426, -COF: 405)

[0229] t: Film thickness (mm)

[0230] Infrared absorption spectrum analysis was performed using a Perkin-Elmer FTIR spectrometer 1760X (manufactured by PerkinElmer) and scanning 40 times. The obtained IR spectrum was automatically determined using Perkin-Elmer Spectrum for Windows Ver. 1.4C, and the 1817 cm -1 and 1884cm -1 The thickness of the film was measured using a micrometer.

[0231] <Loss modulus (G") and storage modulus (G')>

[0232] The pellets of fluororesin obtained in the example were used and compression molded at 210°C to form sheets with a thickness of 2 mm for the measurement of melt viscoelasticity. The fixture used for the measurement used a 25Φ parallel plate, and the sample was set in the melt viscoelasticity measuring device at 210°C. It should be noted that the thickness during the measurement was 0.8 mm. The measurement was performed every 30 seconds at a strain of 0.1% and 10 rad / second, while heating from 210°C to 300°C at a rate of 2°C / minute. The loss modulus at the time of reaching 270°C was recorded as G" 270 , the storage modulus is recorded as G' 270 In addition, the loss modulus at 280°C is recorded as G” 280 , the storage modulus is recorded as G' 280 .

[0233] Example 1 (Production of Fluororesin A)

[0234] 380L of distilled water was added to the autoclave, and after nitrogen replacement, 166kg of octafluorocyclobutane, 83kg of HFP, and 0.3kg of perfluoro(1,1,5-trihydro-1-pentene) (CH2=CF(CF2)3H) were added, and the system was maintained at 35°C and the stirring speed was 200rpm. After that, TFE was pressed into the autoclave to 0.87MPa, and Et was further pressed into the autoclave to 0.95MPa, and then 6.3kg of di-n-propyl peroxydicarbonate was added to start polymerization. Since the pressure in the system decreased as the polymerization proceeded, a mixed gas of TFE / Et / HFP=46 / 44 / 10 mol% was continuously supplied to maintain the pressure in the system at 0.95MPa. In addition, perfluoro(1,1,5-trihydro-1-pentene) was continuously added in a manner that the total amount reached 3.2kg, and stirring was continued for 23 hours. After the pressure was released and returned to atmospheric pressure, the reaction product was recovered.

[0235] The obtained reaction product was washed and dried to obtain 250 kg of a powdery fluororesin. The powdery fluororesin was molded using a single-screw extruder to obtain pellets of fluororesin A.

[0236] Fluororesin A has the following physical properties.

[0237] TFE / ethylene / HFP / perfluoro(1,1,5-trihydro-1-pentene) copolymer

[0238] TFE / ethylene / HFP / perfluoro(1,1,5-trihydro-1-pentene)=45.5 / 44.4 / 9.5 / 0.6 (mol%)

[0239] Melting point: 197°C

[0240] Melt flow rate (265°C): 28.9 g / 10 min

[0241] Number of carbonate groups and carboxylic acid fluoride groups: 314 / 10 6 C

[0242] Loss modulus at 270°C (G”) 270 ):11815Pa

[0243] Difference (G”) 270 -G" 280 ):4455Pa

[0244] Storage modulus (G') at 270℃ 270 ):5058Pa

[0245] Difference (G' 270 -G' 280 ):2148Pa

[0246] The following describes a laminate obtained by using the pellets of the produced fluororesin A. The physical properties of the laminate were measured by the following methods.

[0247] <Adhesion Strength>

[0248] A 1 cm wide sample was cut from the tube obtained in each example and subjected to a 180° peel test at a speed of 25 mm / min using a Tensilon universal testing machine. The average of the five maximum points in the elongation-tensile strength curve was determined as the bonding strength (N / cm).

[0249] <Surface roughness Ra>

[0250] The tube obtained in each example was cut to prepare a test piece, and the surface roughness Ra of the portion of the test piece corresponding to the inner surface of the tube was measured. Using a surface roughness measuring machine (SURFTESTSV-600 manufactured by Mitutoyo), the measurement was repeated three times at 5 points in accordance with JIS B0601-1994, and the average value of the measured values ​​was taken as the surface roughness Ra.

[0251] <Uneven thickness>

[0252] The thickness of the tube obtained in each example was measured at 10 locations at random every 1 m using a micrometer. The ratio (%) of the difference between the maximum and minimum values ​​of the measured thickness to the maximum value of the thickness was calculated (=[(maximum value)-(minimum value)] / (maximum value)×100).

[0253] In the examples, in addition to the fluororesin A, the following materials were used.

[0254] Polyamide 12

[0255] Daicel-Evonik, Vestamid X7297

[0256] Polyamide 612

[0257] Daicel-Evonik, Vestamid SX8002

[0258] Ethylene / vinyl alcohol copolymer resin

[0259] Made by KURARAY, F101B

[0260] Examples 2 to 3 (Production of Laminated Body)

[0261] Using a two-layer tube extrusion device equipped with multiple flow channels (manufactured by PLABOR Research Laboratory of Plastics Technology Co., Ltd.), layer (B) was polyamide 12 and layer (A) was fluororesin A, and they were supplied to two extruders respectively, and two kinds of two-layer multilayer tubes with an outer diameter of 8 mm and an inner diameter of 6 mm were formed according to the extrusion conditions shown in Table 2. The multilayer tube has a layer structure of layer (A) / layer (B), and layer (A) is the innermost layer. The evaluation results are shown in Table 2.

[0262] Examples 4 to 5 (Production of Laminated Body)

[0263] Using a 5-layer tube extrusion device equipped with multiple flow channels (manufactured by PLABOR Research Laboratory of Plastics Technology Co., Ltd.), layer (E) was polyamide 12, layer (B, D) was polyamide 612, layer (C) was ethylene / vinyl alcohol copolymer resin, and layer (A) was fluororesin A, and they were supplied to 5 extruders respectively, and 5 types of 5-layer multilayer tubes with an outer diameter of 8 mm and an inner diameter of 6 mm were formed according to the extrusion conditions shown in Table 2. The multilayer tube has a layer structure of layer (A) / layer (B) / layer (C) / layer (D) / layer (E), and layer (A) is the innermost layer. The evaluation results are shown in Table 2.

[0264] [Table 2]

[0265] Table 2

[0266]

Claims

1. A laminate comprising a fluororesin layer containing a fluororesin and a non-fluororesin layer containing a non-fluororesin, wherein the fluororesin is a fluororesin having a reactive functional group, in, The loss modulus G of the fluororesin at 270°C 270 The loss modulus G of the fluororesin at 280°C 280 The difference G 270 -G" 280 More than 2500Pa, The non-fluorine resin layer includes a polyamide resin layer containing only a polyamide resin as a resin and an EVOH layer containing an ethylene / vinyl alcohol copolymer (EVOH) resin. The fluororesin layer is directly bonded to the polyamide resin layer, and the polyamide resin layer is directly bonded to the EVOH layer.

2. The laminate according to claim 1, in, The storage modulus G' of the fluororesin at 270°C 270 The storage modulus G' of the fluororesin at 280°C 280 Difference G' 270 -G' 280 It is above 1500Pa.

3. The laminate according to claim 1 or 2, in, The fluororesin is a melt-processable fluororesin.

4. The laminate according to claim 1 or 2, in, The fluororesin contains ethylene units and tetrafluoroethylene units.

5. The laminate according to claim 4, in, The fluororesin further contains a hexafluoropropylene unit.

6. The laminate according to claim 1 or 2, in, The number of reactive functional groups of the fluororesin is relative to every 10 6 The number of carbon atoms in the main chain is 3 or more.

7. The laminate according to claim 1 or 2, in, The interlayer bonding strength between the fluororesin layer and the polyamide resin layer is 30 N / cm or more. 8 . A multi-layered tube formed of the laminate according to claim 1 .

9. The tube according to claim 8, in, The inner surface of the tube is formed of the fluororesin, and the surface roughness Ra of the inner surface is 1.0 μm or less.

10. The tube according to claim 8, in, The difference between the maximum value and the minimum value of the thickness of the tube is 5% or less with respect to the maximum value of the thickness.

11. A method for producing a pipe, which is the method for producing a pipe according to any one of claims 8 to 10, in, The tube is obtained by molding the fluororesin at a line speed of 15 m / min or more.

Citation Information

Patent Citations

  • Carbon fibril, its production and composition containing same

    JP1991174018A

  • Ethylene / tetrafluoroethylene copolymer

    JP2019090013A

  • Fluorochemical adhesive material and laminate made with the same

    WO1999045044A1

  • Process for producing multilayered product

    WO2001070485A1

  • Chlorotrifluoroethylene copolymer

    WO2005100420A1